Hao-Yu
Zhao
ab,
Chao
Shu
a,
Peng
Min
b,
Changjun
Li
a,
Wenchao
Deng
b,
Jing
Yang
c,
Xiaofeng
Li
*a and
Zhong-Zhen
Yu
*b
aBeijing Key Laboratory of Advanced Functional Polymer Composites, Beijing University of Chemical Technology, Beijing 100029, China. E-mail: xfli@mail.buct.edu.cn
bState Key Laboratory of Organic-Inorganic Composites, College of Materials Science and Engineering, Beijing University of Chemical Technology, Beijing 100029, China. E-mail: yuzz@mail.buct.edu.cn
cCollege of Chemistry and Chemical Engineering, Hunan Normal University, Changsha 410081, China
First published on 5th October 2022
Although organic phase change materials can reversibly store and release latent heat during their phase change processes, their weak solar–thermal conversion ability, low thermal conduction, and poor structural stability seriously hinder their applications for solar–thermal energy conversion as well as thermal energy utilization. Herein, anisotropic high-quality conical graphene aerogels (HCGAs) with concentric annular structures are constructed to enhance thermal conduction, solar–thermal energy conversion, and shape stability of phase change materials for solar–thermal–electric energy conversion applications. By regulating the orientation of graphene oxide liquid crystals, the resultant graphene sheets are aligned from the apex to the bottom of the cone, providing efficient heat transfer along the vertical direction of the phase change composites. An optimal HCGA/tetradecanol phase change composite with 7.05 wt% of graphene achieves a high through-plane thermal conductivity of 4.54 W m−1 K−1 with a high latent heat of 206.1 J g−1. Benefiting from the larger solar light-absorption surface than conventional square/cylindrical phase change composites and the rapid heat transfer of the anisotropic high-quality graphene conduction network, the conical phase change composite achieves a high solar–thermal energy conversion and storage efficiency of 84.0%. Furthermore, a solar–thermal–electric generator is assembled with the conical phase change composite array, exhibiting maximum output voltages of 261 and 1214 mV under solar light intensities of 100 and 500 mW cm−2, respectively. Even after the removal of the solar light, the voltage output can still be continued by releasing the stored thermal energy.
The drawbacks of the organic phase change materials can be solved by compounding with three-dimensional (3D) graphene aerogels as highly thermally conductive skeletons.21–24 The continuous thermal conduction pathways of the graphene aerogels can significantly enhance the thermal conductivity of phase change materials,25 thereby improving the thermal energy storage and release rates. Moreover, the black graphene sheets exhibit high solar light absorption and satisfactory solar–thermal energy conversion efficiency.26,27 In addition, the hydrophobic and porous graphene skeleton can adequately accommodate phase change materials and suppress their leakage, improving shape stability of the phase change materials.28–30
The two-dimensional graphene sheets with high thermal and electrical conductivities31–34 can be aligned anisotropically to form anisotropic graphene aerogels for enhancing heat transfer along one specific direction of the phase change composites.35–39 As an example, Min et al. fabricated an anisotropic aerogel of high-quality graphene by unidirectionally freezing an aqueous suspension of polyamic acid salt and graphene oxide (GO) sheets to form vertically aligned monolith, followed by freeze-drying, imidization of polyamic acid salt at 300 °C, and graphitization at 2800 °C. The fabricated graphene aerogel/paraffin wax phase change composite exhibits a highly anisotropic thermal conductivity of 8.87 W m−1 K−1 with an exceptional latent heat retention of ∼98.7%.14 An et al. reported a vertically aligned graphene hybrid foam with a concentric circular structure by hydrothermal reduction of GO in the presence of high-quality graphene nanoplatelets (GNPs) followed by air-drying and graphitization, and its epoxy composite possesses an ultrahigh through-plane thermal conductivity of 35.5 W m−1 K−1.40 Apparently, anisotropic graphene aerogels are well suitable for increasing thermal conductivities of phase change composites along the vertical direction, allowing phase change composites to have higher energy storage and release rates for solar–thermal energy conversion and storage, and enabling the phase change composites to be more homogeneous in temperature and phase state during the solar–thermal energy conversion and storage.
Solar–thermal conversion phase change composites can be assembled with temperature-difference power-generation-sheets to form solar–thermal–electric (STE) generators for realizing solar–thermal–electric energy conversion and enhancing the solar energy utilization.41–47 Yang et al. assembled a GNP/boron nitride/polyethylene glycol phase change composite with a power-generation-sheet to obtain a STE generator with a maximum output voltage of ∼123 mV under a simulated solar light irradiation of 400 mW cm−2.48 Cao et al. used GO-enhanced phase change composites for solar–thermal energy conversion, and the maximum output voltage of the STE generator reached 144 mV under a solar light intensity of 200 mW cm−2.49 Liu et al. applied the convex lens to a STE generator, and the maximum power density could be up to 40.28 W m−2 under real sunlight irradiation.15 Currently, considerable efforts are devoted to improving the output voltage and power density of STE generators.
When graphene aerogel-based phase change composites are used for solar–thermal–electric conversion, their cylindrical/square shapes have obvious drawbacks. The lower temperature of the bottom of a phase change composite than that of its top surface due to the top-down input of the thermal energy, the heat dissipation by the large side area of the phase change composite, and the heat loss during the heat transfer50 would unfavorably decrease the temperature difference between the hot and cold source sides of the power-generation-sheets, causing low output voltages.51
To avoid the drawbacks of conventional cylindrical/square-shaped phase change composites, we design high-quality conical graphene aerogels (HCGAs) with concentric annular structures by controlling the orientation of GO liquid crystals during the hydrothermal self-assembly of aqueous GO/GNP suspensions followed by freeze-drying and graphitizing at 2800 °C. Subsequently, the thermally conductive HCGA/tetradecanol phase change composites are fabricated by compounding HCGAs with molten tetradecanol using a vacuum-assisted impregnation approach. At an initial GO/GNP mass ratio of 1:2, the HCGA/tetradecanol phase change composite exhibits a high thermal conductivity of 4.54 W m−1 K−1 at the graphene content of 7.05 wt%. Benefiting from the low graphene loading, the phase change composite achieves a high phase change enthalpy of 206.1 J g−1 and a high latent heat retention rate of 94.5%, indicating its excellent energy storage performance. Because the entire conical surface can be used for solar light absorption and solar–thermal energy conversion, the conical phase change composite has an excellent solar–thermal conversion performance with a solar–thermal conversion and storage efficiency of 84.0%. By assembling the 3 × 3 array of the conical phase change composites with a thermoelectric device, the resultant STE generator under the circumstance of dissipating heat in the air exhibits maximum output voltages of ∼261 and ∼1214 mV under solar light intensities of 100 and 500 mW cm−2, respectively. Even after the removal of the solar light, the voltage output can be continued by releasing the stored thermal energy. Different heat dissipation environments are adopted to enhance the performances of the STE generator, and the potential applications of the solar–thermal–electric energy conversion device are explored.
Fig. 1 Schematic illustrating the fabrication process of conical HCGA skeleton and its thermally conductive tetradecanol phase change composite. |
To prepare a conical hydrogel with anisotropically aligned RGO sheets, the large GO sheets used in the aqueous GO/GNP/KOH suspension with a GO concentration of 5 mg mL−1 can form GO liquid crystals, resulting in the anisotropic arrangement of GO sheets.53 The presence of KOH could bring about electrostatic repulsion between GO sheets, and the mutual exclusion between the GO sheets allows them to align along the inner surface of the mold,54 forming the conical structure with concentric annular orientation in the horizontal direction, and the GO sheets are arranged from the apex to the bottom of the cone along the vertical direction (Fig. 1). During the hydrothermal process, the GO sheets are partially reduced to RGO sheets, and the restored π–π conjugation interactions of RGO sheets enable them to assemble into a 3D network,55,56 and the dispersed GNP sheets have to be distributed inside the RGO skeleton.40
Fig. 2a and b show digital photographs of HCGA2 skeleton and HCGA2/tetradecanol phase change composite. Both HCGA2 and its tetradecanol phase change composite are in black color, beneficial for effective solar light absorption. SEM images (Fig. 2c–f) confirm the concentric annular conical aerogel microstructure of HCGA2. The graphene walls in the HCGA2 tend to orientate concentrically and annularly in the horizontal direction with a layer spacing of ∼10 μm, and the GNPs are uniformly distributed in the skeleton (Fig. 2c and d), while the HCGA2 exhibits the alignment of the graphene sheets from the apex to the bottom of the cone in the vertical direction (Fig. 2e and f). In addition, the low magnification SEM images clearly show the concentric circular arrangement of the graphene sheets in the horizontal direction (Fig. S3†). It is also seen that the graphene walls are not separate but bridged by graphene sheets, demonstrating the formation of 3D interconnecting graphene networks, which facilitates heat transfer in both vertical and horizontal directions. Digital photographs of the cross-section of HCGA2 also demonstrate the concentric circular orientation trend of the graphene sheets in the horizontal direction, and its side-section photograph confirms the orientation in the vertical direction (Fig. S4a–c†). In addition, the bottom photograph of the HCGA2/tetradecanol shows the concentric circular orientation of the graphene sheets inside the phase change composite (Fig. S4d†).
Fig. 2 Digital photographs of (a) HCGA2 and (b) HCGA2/tetradecanol phase change composite. SEM images of (c, d) cross-section and (e, f) side-section of the conical HCGA2. |
To monitor the evolution of graphene quality during the fabrication process, Fig. 3 shows Raman mapping images of GO, RGO, GNP, CGA2 and HCGA2. As shown in Fig. 3a–e, the color of the area close to blue indicates a low intensity ratio of D and G bands (ID/IG) and a low defect density of sheets, while the color close to red implies a high ID/IG value and a high defect density. The colors of the Raman mappings of GO and GNP are uniform (Fig. 3a and c), demonstrating the stable quality of the raw materials. In particular, the Raman mapping of GNP is dark blue, reflecting its excellent quality.
The comparison of Fig. 3b with Fig. 3a reveals the increase in the defect density after hydrothermal treatment of GO due to the removal of oxygen-containing functional groups on GO.57 The uneven color of the Raman mapping of CGA2 (Fig. 3d) derives from the presence of RGO and GNP with a significant difference in defect density. After graphitizing at 2800 °C in an inert atmosphere, in contrast, the Raman mapping of HCGA2 exhibits uniform dark blue (Fig. 3e), verifying that the high-temperature thermal annealing can heal the defects of the RGO and hence improve the quality of graphene in the aerogel.58Fig. 3f enumerates the average ID/IG values of the Raman mapping regions of GO, RGO, GNP, CGA2 and HCGA2. The ID/IG values of GO, RGO and CGA2 are in a high range, indicating that more defects exist on the graphene sheets without the high-temperature annealing treatment, which would cause serious phonon scattering at the defect regions and result in heat loss.59 On the contrast, HCGA2 exhibits an extremely low ID/IG value, which is the reflection of its high quality of graphene sheets and implies the greatly enhanced heat conduction of the HCGA2 skeleton.
Fig. 4a manifests XRD patterns of GO, GNP, CGA2, and HCGA2. The GO exhibits a typical diffraction peak at ∼12°, reflecting its layer spacing of ∼0.74 nm,60 much larger than that of pristine graphite of 0.34 nm, because of the oxygen-containing functional groups on the lamellae of GO; whereas, the GNP shows a sharp peak at 26.4°, corresponding to a layer spacing of 0.34 nm. The disappearance of the typical diffraction peak of GO and the appearance of a sharp peak at 26.4° in the XRD patterns of CGA2 and HCGA2 demonstrate that the hydrothermal treatment and the high-temperature graphitization can sufficiently remove the oxygen-containing groups of GO sheets.61
To confirm the influence of the anisotropic structure of the aerogels on the through-plane thermal conductivity, the iHCGA2/tetradecanol phase change composite with a random arrangement of graphene sheets is fabricated for comparison, and its thermal conductivity is 3.76 W m−1 K−1, lower than that of the HCGA2/tetradecanol counterpart, indicating that the orientation of the graphene sheets in the vertical direction is positive for the enhancement in through-plane thermal conductivity of the phase change composite. In addition, the positive contribution of the graphitization is well reflected by the fact that the thermal conductivity of the HCGA2/tetradecanol is 3.65-fold of the CGA2/tetradecanol in the absence of the graphitization. The TGA analysis reveals that the total graphene/GNP content in the graphene aerogel/tetradecanol composites increases with the GNP content. The loading of graphene/GNP in the HCGA2/tetradecanol is ∼7.05 wt% (Fig. 4c), which is still at a low loading level.41,48,67,68
Fig. 4d and e show DSC curves of tetradecanol, HCGA1/tetradecanol, and HCGA2/tetradecanol. The comparison of these curves indicates that the peak shapes and peak positions of the graphene aerogel/tetradecanol composites are almost identical to those of the tetradecanol during the heating and cooling processes, demonstrating that no chemical reaction occurs between the graphene aerogel and tetradecanol during the compounding process.69 Notably, there are two obvious exothermic peaks during the cooling of tetradecanol and graphene aerogel/tetradecanol phase change composites, representing the liquid–solid transition and the solid–solid transition.70 Table S1† lists the melting temperature (Tm), melting enthalpy (ΔHm), crystallization temperature (Tc), and crystallization enthalpy (ΔHc) of tetradecanol and its phase change composites. HCGA2/tetradecanol has a Tm of 35.8 °C, which is very close to that of tetradecanol (35.6 °C), indicating that the introduction of HCGA2 hardly affects the phase transition behaviour of tetradecanol.71 On the basis of the ΔHm of tetradecanol (218.0 J g−1), the ΔHm of HCGA2/tetradecanol is calculated to be 206.1 J g−1 with a high latent heat retention rate of 94.5%, which is ascribed to the low graphene/GNP loading in the HCGA2/tetradecanol. Moreover, the DSC curves of the HCGA2/tetradecanol after 50 and 100 heating–cooling cycles almost coincide with the first cycle (Fig. S5†), indicating that the phase change composite possesses excellent cyclic stability in terms of thermophysical properties and high reliability in long-cycle operation.
As the introduction of graphene could cause the decrease in phase change enthalpy of the phase change materials, the high graphene loading would compromise the energy storage capacity of the phase change composite.13 By promoting the quality of graphene and controlling the graphene loading at a low level, the HCGA2/tetradecanol has an excellent thermal conductivity while retaining a high phase change enthalpy of the tetradecanol matrix. Fig. 4f shows the thermal conductivities and latent heat retention rates of phase change composites reported in recent years.8,15,27,30,41,67,71–74 Apparently, the HCGA2/tetradecanol possesses a relatively high thermal conductivity and an outstanding latent heat retention rate, which is well suitable for solar–thermal energy conversion and thermal energy storage.
Besides, the higher temperature of the bottom of the HCGA2/tetradecanol that contacts the hot side of the power-generation-sheet is favorable for improving the output voltage of the STE generator.76 The solar–thermal conversion and thermal energy storage efficiency (λ) of a phase change composite is calculated by the equation: λ = (m × ΔH + m × Cp × ΔT)/(P × A × t), where m, ΔH, and Cp are the mass, melting enthalpy, and specific heat capacity of the phase change composite, respectively. ΔT is the temperature increase during the melting process, P is the solar light intensity, A is the projected area of the light-receiving surface, and t is the duration of the melting process. The beginning and ending positions of the melting process are determined by a linear fitting method (Fig. S7†). As calculated, the λ of the HCGA2/tetradecanol is up to 84.0% under a light intensity of 100 mW cm−2.
For comparison, the solar–thermal conversion performances of the cylindrical HGA2/tetradecanol under the same light intensity (100 mW cm−2) are characterized, and its temperature–time curves are shown in Fig. 5e. In the irradiation process, as the lower part of the cylindrical HGA2/tetradecanol cannot receive the solar light, the heat can only be generated by the upper surface and transferred to the lower part of the sample, during which the heat loss occurs inevitably. Different from the HCGA2/tetradecanol, the HGA2/tetradecanol cannot keep the lower part at a high temperature. As the smaller effective surface area of the HGA2/tetradecanol than that of the HCGA2/tetradecanol, and the inevitable heat dissipation from the side surface of the HGA2/tetradecanol to the environment, the λ of HGA2/tetradecanol is only 75.2%. The beginning and ending positions of the melting process are determined by a linear fitting method (Fig. S8†), and the maximum temperature is ∼49 °C. Clearly, the conical shape endows the HCGA2/tetradecanol with a better solar–thermal conversion performances. As a comparison experiment, the temperature of the conical tetradecanol is measured under the light intensity of 100 mW cm−2 (Fig. S9†). The maximum temperature of the tetradecanol is only ∼34 °C, and its phase transition cannot occur, leading to no heat storage. These results confirm that the solar–thermal conversion of tetradecanol is improved remarkably by the HCGA2. Fig. 5f compares the light absorbances of the HCGA2/tetradecanol and tetradecanol in the whole wavelength range of 250–2500 nm. The absorbance of HCGA2/tetradecanol remains almost above 85%, much higher than that of tetradecanol, indicating the excellent light absorption ability of the HCGA2/tetradecanol.
Fig. 6b shows the temperature–time curves of the phase change composites under a light intensity of 100 mW cm−2. When the aluminum fins are placed in the air, under the solar light irradiation, the temperature of the phase change composites rises to the phase change temperature, and the phase transition occurs to achieve the heat storage. The maximum temperature of the phase change composite is ∼45 °C because a part of the heat converts to electrical energy, and a part of the heat transfers to the aluminum fins via the power-generation-sheet and dissipates to the environment. The red curve in Fig. 6d is the output voltage–time curve of the STE generator for dissipating heat in the air under a light intensity of 100 mW cm−2. In the initial irradiation stage (Stage a), the temperature of the phase change composites rises rapidly, resulting in an increase in the temperature difference between the hot and cold source sides of the power-generation-sheet and a sharp rise in the output voltage. The temperature of the phase change composites is almost constant during the phase transition, but the heat still transfers to the cold side of the power-generation-sheet, causing the decrease in temperature difference between the hot and cold sides, and hence the output voltage tends to drop in Stage b. After completing the phase transition of the phase change composites, the temperature rises rapidly again, resulting in a sharp increase in output voltage (Stage c). Subsequently, the device reaches a stable state of the temperature and the output voltage (Stage d).
After stopping the solar light irradiation, the output voltage of the STE generator drops steeply due to the absence of the energy input (Stage e). As the temperature of the phase change composites remains constant after dropping to the solidification platform while the aluminum fins are still dissipating heat, the temperature difference between the hot and cold sides of the power-generation-sheet still increases, leading to the increase in output voltage in the absence of solar light (Stage f). This result demonstrates that the released thermal energy from the phase change composite can be converted to electrical energy. Similarly, the second output voltage rise (Stage g) is achieved by releasing the energy at the second solidification platform. Finally, the phase change composite is gradually cooled to room temperature, and the STE generator stops outputting voltage (Stage h). The voltage–time curves demonstrate that the STE generator can still output voltage for 2100 s in the absence of the solar light after the solar light irradiation for 2400 s under a light intensity of 100 mW cm−2 when the aluminum fins are placed in the air. The storage and release energy capability of the phase change composites is crucial for endowing the STE generator to output voltage continuously at the daytime and night. The maximum output voltage can be up to ∼261 mV. In the other two heat dissipation environments, as a large amount of heat is absorbed by the environments, the temperature of the phase change composite cannot reach the phase change temperature, and the latent heat of the phase change composite cannot be utilized for heat storing and releasing, which is reflected in the rapid voltage drop after stopping the solar light irradiation.
Furthermore, when the STE generator is exposed to a high light intensity of 500 mW cm−2, the temperatures of the phase change composite and the output voltages of the STE generator are measured (Fig. 6c and e). Thanks to the large improvement in the input energy, the temperature of the phase change composite can reach the phase change temperature in all three heat dissipation environments, and the STE generators can still output the voltage for some time after stopping the solar light irradiation. Fig. S11 and S12† manifest the output voltage and output current curves for all working environments, demonstrating that the voltage and current have the same trend. Fig. 6f and g compare the maximum output voltage, output current, output power, and power density of STE generators in the three heat dissipation environments under light intensities of 100 and 500 mW cm−2. The highest output voltage of ∼330 mV is achieved when the heat dissipation environment is the ice water at the light intensity of 100 mW cm−2, which is attributed to the largest temperature difference between the hot and cold sides of the STE generator when the aluminum fins are placed in the ice water. The output power and power density of the STE generator under this condition can reach 11.9 mW and 4.20 W m−2, respectively. When the light intensity increases to 500 mW cm−2, the phase change composite can receive more solar energy and convert it to heat energy, resulting in a particularly high temperature; whereas, the aluminum fins still maintain a low temperature by dissipating the heat in the water. The resultant large temperature difference between the hot and cold sides of the power generator sheet leads to a maximum output voltage of the STE generator (∼1214 mV). The output power of the STE generator under this working condition can reach 138.8 mW with a power density of 49.08 W m−2. Table S2† manifests that the maximum output voltage and current of the STE generators are much higher than those reported at the same light intensities.47 Even at low light intensities, the maximum output voltage and current of the STE generators are superior to the reported performances at high light intensities.41,42,44,47–49
To demonstrate a practical application, the STE generator is exposed to light with an intensity of 1200 mW cm−2, and served as a power supply for an external circuit, which enables LED bulbs to emit light (Video S1†), and the measured voltage can be ∼2.02 V (Fig. S13†). Actually, the enhanced light intensities can be readily achieved in practical application scenarios by concentrating solar beams with convex lenses and concave mirrors.78,79 In addition, the heat dissipation condition of the ice/water mixture simulates the use of the STE generator in cold environments (e.g., high-latitude regions, and high-altitude glacier areas), confirming the feasibility of the STE generator for solar–thermal–electric energy conversion in such cold regions.
Footnote |
† Electronic supplementary information (ESI) available: AFM images and height profile of GO and GNPs; SEM images and digital photographs of the samples; Tm, ΔHm, Tc and ΔHc of the samples; DSC curves of HCGA2/tetradecanol after heating–cooling cycles; temperature difference between the bottom and top of HCGA2/tetradecanol during the solar–thermal energy conversion; determination of the beginning positions and ending positions of the melting processes of HCGA2/tetradecanol and HGA2/tetradecanol; temperature–time curves of the bottom of HCGA2/tetradecanol and tetradecanol; schematic of the components in the solar–thermal–electric energy conversion measurements; voltage–time curves and current–time curves of STE generators; digital photographs of LED bulbs lit by the STE generator and the output voltage; comparison of maximum output voltages and output currents of the STE generators in this work with those reported in the literature. See DOI: https://doi.org/10.1039/d2ta06457j |
This journal is © The Royal Society of Chemistry 2022 |