Open Access Article
Chiara Maccato
*ab,
Davide Barreca
*b,
Lorenzo Signorina,
Enrico Scattolin
a,
Gloria Tabacchi
c,
Ettore Fois
c,
Cinzia Sada
d,
Oleg I. Lebedeve,
Alberto Gasparotto
ab,
Evgeny Modinf,
Ermanno Pierobona,
Naida El Habrag and
Gian Andrea Rizziab
aDepartment of Chemical Sciences, Padova University and INSTM, 35131 Padova, Italy. E-mail: chiara.maccato@unipd.it
bCNR-ICMATE and INSTM, Department of Chemical Sciences, Padova University, 35131 Padova, Italy. E-mail: davide.barreca@unipd.it
cDepartment of Science and High Technology, Insubria University and INSTM, 22100 Como, Italy
dDepartment of Physics and Astronomy, Padova University and INSTM, 35131 Padova, Italy
eLaboratoire CRISMAT, UMR 6508 CNRS/ENSICAEN/UCBN, 14050 Caen Cedex 4, France
fCIC nanoGUNE BRTA, 20018 Donostia, San Sebastian, Spain
gCNR-ICMATE, 35127 Padova, Italy
First published on 26th September 2025
Electrocatalytic oxygen evolution reaction (OER), playing a key role in water splitting processes to yield green hydrogen, is critically dependent on the implementation of stable, efficient, and economically viable catalysts. Among the various runners, NiO-based nanomaterials have recently gained considerable attention. Herein, we focus on the plasma enhanced-chemical vapor deposition (PE-CVD) of NiO nanoarchitectures, grown on conducting glasses from a fluorinated Ni(II) precursor and subjected to a comprehensive experimental and theoretical characterization. Modulations of the growth temperature from 100 to 400 °C yielded a progressive evolution from hierarchical quasi-1D nanopillars, featuring the surface presence of CFx groups, to cauliflower-like structures, characterized by a homogeneous fluorine distribution inside NiO. The open morphology of the 100 °C-grown system, possessing a higher content of structural defects, enhanced charge carrier transport and promoted reactants/products diffusion, yielding the best activity among the investigated materials (overpotential of ≈390 mV at 10 mA × cm−2 and Tafel slope of 39 mV × dec−1). Density functional theory (DFT) modeling indicates that CFx groups create intra-gap empty states which could promote OER activity. The obtained performances compare favorably with various Ni-based electrocatalysts reported up to date, opening the door to additional research developments towards sustainable energy generation.
Over the last years, we have reported on the vapor phase synthesis of first-row transition metal oxide films/nanostructures from fluorinated diketonate-diamine molecular precursors [M(β-dik)2TMEDA, with M = Mn,33–37 Fe,38–40 Co;18,41,42 β-dik = tfa (1,1,1-trifluoro-2,4-pentanedionate) or hfa (1,1,1,5,5,5-hexafluoro-2,4-pentanedionate), and TMEDA = N,N,N′,N′-tetramethylethylenediamine]. The results demonstrated that, under suitable conditions, these compounds act as single-source molecular precursors for both M and F, yielding materials with a tunable fluorine content. For electrocatalytic applications, low temperature plasma technology43 and, in particular, plasma enhanced-chemical vapor deposition (PE-CVD), are efficient and flexible fabrication methods,5 thanks to the possibility of yielding nanosystems with unique properties under non-equilibrium conditions. Up to date, only a few works have been dedicated to the PE-CVD of nickel(II) oxide materials.44–46
Basing on preliminary results,31 we report herein on the PE-CVD of NiO nanomaterials on fluorine-doped tin oxide (FTO) glass substrates from Ni(tfa)2TMEDA, already used as a precursor in the thermal CVD of nickel(II) oxide.47 The present materials, grown at different temperatures (Fig. 1), were subjected to a thorough characterization, supported by density functional theory (DFT)-based calculations. Interestingly, this approach enabled the simultaneous control of material morphology, chemical composition, microstrain, and dislocation density. Indeed, the last two parameters are pivotal in tailoring the properties of nanostructured systems48 and, in particular, the molecular interactions between reactants and catalytic surfaces, enhancing thus the ultimate OER activity.49 The best performances, well positioned in the panorama of NiO-based OER electrocatalysts, were obtained for the systems grown at 100 °C, the lowest ever reported up to date in the PE-CVD of nickel(II) oxide.44–46 In perspective, the outcomes of the present study can be beneficial for the design of efficient and low-cost catalyst systems based on transition metal oxides.
![]() | ||
| Fig. 1 Schematic representation of the route adopted in the present work for the synthesis of NiO electrocatalysts on FTO substrates. | ||
m).50 Consistently with the face-centered cubic (fcc) nickel(II) oxide lattice, the observed reflections obeyed selection rules with Miller indexes (hkl) being either all even, or all odd.47 Relative peak intensities were found to depend on the adopted growth temperature (see also the SI, S3). The average crystallite sizes underwent a progressive increase at higher substrate temperatures, i.e. upon enhancing the thermal energy supply (Fig. 2a, inset),51 similarly to the case of MnO2 nanosystems obtained via PE-CVD starting from an analogous molecular precursor.37 The microstrain (ε) and dislocation density (δ) values [calculated using eqn. (S2) and (S3), SI] are plotted in Fig. 2b and c. In general, δ and ε values are directly dependent not only on material fabrication route, but also on the processing conditions.47 In the present case, δ and ε values decreased for higher crystallite dimensions, in line with previous studies.47,51,52 Dislocation density values were compatible with those reported for NiO films obtained by sputtering on Si(100) and glass substrates.51–53 Altogether, these results indicated that a lower growth temperature is correlated to a larger content of structural defects.37 As discussed below, the highest microstrain and dislocation density values obtained for the specimens grown at 100 and 200 °C directly contribute to the enhanced functional performances of these catalysts in comparison to the 300 °C and 400 °C-grown samples.
The system chemical composition was investigated by X-ray photoelectron spectroscopy (XPS), that yielded qualitatively similar results regardless of the adopted growth temperature. Wide-scan spectra (Fig. 3a) displayed the presence of C (see the related comments in the SI, as well as Fig. S3 and Table S1), O, Ni, and F photopeaks. A weak Sn 3d signal (corresponding to ≈0.2 at% of tin) was present only for the specimen grown at 100 °C, in accordance with the corresponding material morphology (see below and Fig. 6). For all the target samples, Ni 2p photoelectron peaks (Fig. 3b and S4 in the SI) presented very similar shapes and energy positions, and were characterized by the absence of features at a binding energy (BE) of 852.5 eV, ruling out the occurrence of metallic Ni.10,28,54 Differently from a simple spin-orbit doublet, these peaks appeared as complex signals characterized by the presence of intense satellites at BEs ≈6 eV higher than the main spin-orbit components. The actual Ni 2p lineshape, directly influenced by multi-electron interactions between the emitting metal center and its nearest neighbors, was typical for the presence of Ni(II) in NiO.2,6,14,32,47,55 The signal could be fitted by means of contributing bands positioned at 853.6 eV, 855.6 eV, 860.5 eV, 862.8 eV, 865.9 eV (j = 3/2), and 871.3 eV, 873.4 eV, 877.1 eV, 880.1 eV, and 883.2 eV (j = 1/2), for whose interpretation the reader is referred to previous works.16,55 At variance with other studies,22 no net evidence of Ni(III) occurrence was obtained from spectral analysis.
![]() | ||
| Fig. 3 (a) Surface wide-scan XPS surveys of NiO samples fabricated at different temperatures. Detailed Ni 2p (b), O 1s (c), and F 1s (d) regions for a specimen grown at 300 °C are also displayed. (e) Evolution of CFx (pink points, left axis) and lattice F contributions (orange points, right axis) as a function of the growth temperature. X(FCFx) and X(Flattice) were calculated as: X(FCFx) = [(at% FCFx)/[(at% FCFx) + (at% Ni)]] × 100 and X(Flattice) = [(at% Flattice)/[(at% Flattice) + (at% Ni)]] × 100.36 | ||
The O 1s photoelectron peaks (Fig. 3c and S5 in the SI) were deconvoluted by two different components, located at 529.8 eV (I) and 531.5 eV (II). The predominant one (I) was ascribed to lattice oxygen in NiO,12,23,31,47 whereas band (II) resulted from the concomitant contribution of hydroxyl and carbonate groups chemisorbed on O defects.21,31,35,47,55,56 A detailed analysis of fitting results (Table S2, SI) revealed a slight increase of band (II) contribution to the overall O 1s signal at expenses of component (I) upon increasing the growth temperature. In parallel, the O/Ni at% ratio underwent a modest decrease from (0.97 ± 0.02) to (0.89 ± 0.02) upon going from the 100 °C to the 400 °C specimen, suggesting thus the formation of NiO featuring a moderate oxygen deficiency.
Recently, oxygen vacancies engineering was applied to boost the OER activities of NiO electrocatalysts via the optimization of the system characteristics.17,28,57 Nevertheless, in the present case the occurring variations are very modest, and cannot significantly contribute to the observed reactivity trend.
The F 1s peak features (Fig. 3d and S6 in the SI) were directly dependent on the adopted deposition temperature. For T ≥ 200 °C, the F 1s signal was characterized by two components, positioned at mean BE = 684.5 eV (III) and 688.2 eV (IV) (Table S3, SI). The former, associated to Ni–F bonds, revealed a successful fluorine incorporation into NiO lattice, yielding thus F-doped NiO nanomaterials,36,58,59 a result enabled by the used fluorinated precursor. Component (IV), ascribed to precursor-derived CFx groups,31,36,42 underwent a progressive decrease at higher growth temperatures (see Fig. 3e, pink curve, and S6, SI). At 100 °C, component (IV) was the only one contributing to the F 1s signal. These trends, displayed in Fig. 3e, underscore the possibility of modulating the nature and content of F-containing moieties in the target NiO nanosystems, enabling a parallel tailoring of OER functional activity (see below).
Additional information on the in-depth composition was obtained by secondary ion mass spectrometry (SIMS; Fig. 4). The average C content in the samples was estimated to be as low as tenths of ppm, suggesting thus a clean conversion of the used precursor into NiO under the adopted conditions. In fact, the ionic yields of nickel and oxygen evidenced an even composition throughout the investigated thickness, irrespective of the adopted growth temperature. The obtained results confirmed the presence of fluorine in all specimens, with an overall average content estimated to be between 130 and 160 ppm, but its in-depth distribution was directly affected by the deposition temperature. Whereas at 100 °C an appreciable decrease of the corresponding signal took place throughout the outermost 400 nm, a more even F spatial distribution could be observed for the specimens grown at 300 °C and 400 °C. These results, in line with XPS (Fig. 3e and S6; Table S3, SI) and TEM outcomes (Fig. 7, 8, S11 and S12, SI), indicate that fluorine is mostly present in the near-surface regions in the form of CFx groups at the lowest growth temperature. In a different way, the more even fluorine in-depth distribution upon increasing the thermal energy supply could be related to the higher lattice F content (see also above). Taken together, these outcomes indicate that, under suitable conditions, Ni(tfa)2TMEDA can be a single-source precursor for the PE-CVD of F-doped NiO, coherently with previous results for Mn3O4,35 MnO2,34,37 Fe2O3,38 Co3O4,42 and NiO.47
![]() | ||
| Fig. 4 SIMS depth profiles of specimens grown at 100 °C (a), 200 °C (b), 300 °C (c), and 400 °C (d). | ||
The electronic properties of the fabricated systems were further investigated by reflection electron energy loss spectroscopy (REELS) and valence band analysis. The recorded REELS spectra (Fig. 5a) showed, beside the intense signal originating from elastic scattering of the incoming electrons centred at zero energy loss, a feature located between 1 and 2 eV, attributable to scattering collisions of the primary beam with hydrogen atoms in the material.31,60 H content appeared to be qualitatively higher at the lowest deposition temperatures (100 °C and 200 °C). The onset of the anelastic background enabled to estimate the material band gap values, that turned out to be all very similar (Table S4, SI) and in line with literature values for NiO obtained by thermal CVD,47 reactive sputtering61 and solution routes.62
Fig. 5b reports the He(I) ultraviolet photoelectron spectroscopy (UPS) valence bands of NiO materials, whereas the corresponding XPS valence bands are displayed in Fig. S7, SI. Table S4, SI reports the extrapolated work function data, together with ionization potential and electron affinity values. The latter, affected in general by the adopted fabrication strategy and processing conditions,47,63 were rather similar for the present materials. The calculated offset values of valence band edges from the Fermi level (EF − VB) underscore, as expected, a p-type conductivity of the target specimens.47 Based on these results, a tentative band scheme for the investigated nanomaterials is proposed in Fig. 5c. As can be observed, variations between the different specimens are quite modest, suggesting that their OER activities (see below, Fig. 9 and related comments) should be rather affected by other parameters and phenomena.
Preliminary morphological analyses were carried out by the combined use of field emission-scanning electron microscopy (FE-SEM) and atomic force microscopy (AFM; Fig. 6), that revealed a direct dependence of material features on the growth temperature. At 100 °C (Fig. 6a), the images were dominated by hierarchical quasi-one dimensional (1D) nanopillars [overall length = (800 ± 10) nm; lateral width = (40 ± 5) nm; aspect ratio = (800/40) = 20 ± 3]. The obtainment of this morphology can be traced back to the electrical field present at the plasma-sample interface, producing the observed anisotropic growth. Each pillar resulted by the aggregation of almost spherical nanoparticles (NPs) with a mean size of (25 ± 5) nm. These results, never reported, to the best of our knowledge, for nickel(II) oxide materials obtained by PE-CVD, underscore the plasma activation role in the formation of the target systems at low deposition temperatures. The assembly of such nanopillars resulted in the formation of an open area system, a favorable feature in view of the ultimate OER end-uses.2,4–7,9 In fact, catalysts based on 1D nanomaterials can be deemed to be more efficient thanks to the large exposed surface and high density of active sites.19
A relatively similar morphology could be observed even for the sample grown at 200 °C (Fig. 6b), although the formation of bigger and denser nanostructures yielded a less open cross-sectional arrangement. The overall deposit thickness underwent a reduction to (520 ± 10) nm, highlighting thus that an increase in the thermal energy supply renders lateral growth progressively competitive with the vertical one. This observation was corroborated by examining FE-SEM micrographs of specimens synthesized at 300 °C and 400 °C (Fig. 6c and d), which featured the interconnection of cauliflower-like structures and turned out to be more packed due to an enhanced lateral diffusion during material growth. For such systems, the deposit thickness was comprised between 470 nm and 500 nm. Cross-sectional line-scan energy dispersive X-ray spectroscopy (EDXS) profiles highlighted a very good compositional homogeneity, as demonstrated by the parallel trends of Ni Kα and O Kα signals throughout the deposit thickness (Fig. S8 and S9, SI). The specimen grown at 400 °C was characterized by F presence throughout the investigated depth, with a signal trend almost parallel to the Ni one (Fig. S9, SI), in line with SIMS results (see above and Fig. 4d). AFM images (Fig. 6, right panel and S10, SI) evidenced a granular surface topography for all systems, with a root-mean-square roughness of (17 ± 2) nm, regardless of the used growth temperature. This latter result could be attributed to the technique incapability of probing the whole material morphology throughout its profile, precluding thus the obtainment of significant differences for the target electrocatalysts.31 In line with these observations, line scan profiles for the different specimens (Fig. S10, SI) were very similar.
In order to investigate in detail the system nanoscale structure, advanced TEM and related analyses were carried out on selected specimens fabricated at the lowest and highest deposition temperatures (Fig. 7 and 8). Low magnification high angle annular dark field-scanning TEM (HAADF-STEM) images and a simultaneously acquired EDXS-scanning TEM (EDXS-STEM) elemental map for the specimen fabricated at 100 °C are reported in Fig. 7a–c. As can be observed, the sample consists of NiO NPs (see also Fig. 7d), interconnected to form hierarchical quasi-1D pillars with an average length of (800 ± 10) nm, oriented almost perpendicularly to the underlying FTO substrate (Fig. 7b). The presence of these structures is consistent with FE-SEM results (Fig. 6). Nanoparticle bundles (200 ÷ 300 nm dimensional range, Fig. 7a), are separated by 50–100 nm voids, resulting thus in a high area nanoarchitecture, favorable for OER end-uses. NiO NPs have a typical average size of (30 ± 5) nm (Fig. 7d and e), and are 〈111〉− and 〈100〉-faceted (Fig. 7f and g).
According to the outcomes of EDXS-STEM analyses (see Fig. 7c and S11, SI), Ni and O are characterized by a homogeneous spatial distribution, and no segregation phenomena could be observed. Furthermore, high magnification and high resolution HAADF-STEM imaging enabled to rule out the occurrence of any secondary phase or amorphous layers at NPs surface and joint boundaries (Fig. 7e and f). These results confirmed the obtainment of cubic nickel(II) oxide (space group: Fm
m50), in accordance with XRD results, with some NiO NPs exhibiting a twinned structure. As a representative case, Fig. 7f and g show an elongated twinned single NiO NP, with a width and length of (20 ± 2) and (40 ± 3) nm, respectively, and 〈111〉 twin planes, as typically observed for cubic structures. These twinnings were present in almost all NiO NPs for the target specimen, irrespective of the specific location.
At variance with the sample grown at 100 °C, presenting quasi-1D pillars, the one grown at 400 °C was characterized by interconnected, multi-granular cauliflower-like structures (Fig. 8a). As already mentioned, this difference was mainly ascribed to the enhanced thermal energy supply at higher substrate temperatures, resulting in the lateral growth being competitive with the vertical one, and leading to a more compact structure with a lower overall thickness [(520 ± 10) nm]. Even at 400 °C, no segregation phenomena or secondary phases could be evidenced, and EDXS-STEM mapping showed a homogeneous nickel and oxygen distribution. However, the 400 °C-grown sample presented an important difference with respect to the one obtained at 100 °C, related to the presence of evenly distributed fluorine (Fig. 8b and S12, SI), in accordance with the results of compositional analyses (see above). Electron diffraction (ED) analyses and bright field-high resolution TEM (BF-HRTEM) imaging (Fig. 8c and d) unambiguously confirmed the presence of cubic NiO as the sole crystalline phase and demonstrated 〈111〉/〈100〉 faceting, similar to the case of the 100 °C-grown specimen.
![]() | ||
| Fig. 9 (a) Photograph of the cell used for electrochemical tests (WE = working electrode; RE = reference electrode; CE = counter-electrode), with an enlargement of WE with the copper tape used for contacting. OER performances of NiO electrodes in alkaline water: (b) LSV curves for the target specimens. The peaks in the potential range 1.4–1.5 V correspond to the formation of NiO(OH),16,17,20,27,28,32 whose occurrence is also supported by ex situ XPS analyses (see below). (c) Corresponding current density values at 1.6 V vs. RHE. (d) Tafel plots (dashed and continuous lines indicate experimental and fitting curves, respectively); (e) TOF vs. overpotential curves. | ||
The best performances of the 100 °C-grown sample in the target electrocatalyst family can be attributed to the synergy of different phenomena. The main one is linked to morphology-related transport properties. Specifically, despite the higher thickness in comparison to the 400 °C-grown electrocatalyst, the 100 °C-grown specimen features a more open structure. Thus, the higher active area favours the access of reactant molecules to Ni active sites and the subsequent product outdiffusion.19,25,58 Accordingly, travel distances of charge carriers are reduced, minimizing thus detrimental electron–hole recombination and yielding an improved OER activity.7 An additional contributing effect relates to the higher microstrain and dislocation density obtained for this specimen. In fact, by disrupting the equilibrium of interatomic bonds at metal sites, a faster adsorption/dissociation kinetics of the incoming oxygen molecules occurs, resulting thus in an improved electrocatalytic activity.49
Another important difference between the target electrocatalysts is related to the different types and relative contents of F-containing moieties. Indeed, as highlighted by compositional data (see above and Fig. 3e), fluorine was present both in Ni-F bonds and in precursor-derived CFx groups, corresponding respectively to components (III) and (IV) in Fig. 3d and S6 in the SI, with (IV) being the only contribution for the sample grown at 100 °C. These CFx groups have a direct influence on electrocatalytic activity, as explained below. Any significant influence of oxygen vacancy content on the different activities of the investigated materials could be unambiguously ruled out, since, as observed above, O/Ni at% ratios were very close for all the target systems.
Results on the catalyst stability, a critical factor in view of eventual real-world applications,11,14,29 are reported in the SI (see Fig. S13 and S14). As can be observed in Fig. S13, SI, after an initial induction period in which the slight current density decrease might be related to the generated O2 bubbles, which did not leave the surface immediately during gas generation,28 both the specimens grown at 100 °C and 400 °C present rather constant performances upon prolonged utilization. On this basis, the occurrence of relevant degradation/poisoning phenomena was ruled out, as also supported by the negligible variations featured by LSV curves (Fig. S14a, SI) and the calculated Tafel slopes after long-term stability tests (Fig. S14b, SI; compare with the values of the pristine electrocatalysts reported in Table S5, SI).
Coherently with the above results, post-operando XRD and FE-SEM investigation after prolonged electrochemical tests evidenced that the system structure and morphology did not undergo appreciable alterations (compare Fig. S16, SI with Fig. 2a and S17, SI with Fig. 6). It is worthwhile noticing that interaction with the KOH electrolyte leads to the surface formation of Ni(OH)2 and NiO(OH),27,32 as indicated by the XPS signals of Ni 2p and O 1s acquired after functional tests. In fact, for both the specimens grown at 100 °C and 400 °C, this conclusion is supported by the Ni 2p lineshape variation and by the intensity increase of component (II) in the O 1s peak (see Fig. S18 and S19, SI).8,16,54 This phenomenon was accompanied by the appearance of band (III) in the O 1s photopeak (see Table S6, SI), related to adsorbed water,8,16,55 as well as by an increase of the CFx contribution to the overall F 1s signal for the 400 °C-grown sample (compare Tables S3 and S7, SI). Nevertheless, the overall fluorine content (≈4 at%) does not show any appreciable decrease after prolonged testing (Fig. S20, SI), enabling thus to rule out any substantial fluorine dissolution during OER. These results are in tune with the above indications and enable to discard any significant long-term performance decay.
To rationalize the obtained results, hydroxylated NiO surfaces exhibiting CFx groups and both reticular F (Fr) and adsorbed CFx groups – mimicking samples grown at T = 100 °C and T > 100 °C, respectively – were modelled (S2 and S6, SI). For sake of completeness, models characterized by different compositions of precursor-derived CFx moieties (namely CF3, CF2, and CF) were initially investigated (Fig. S1, SI). Only the CF-containing models featured properties compatible with the p-type nature of the deposited materials (Table S9 and Fig. S22, SI), suggesting therefore that the most likely composition of CFx moieties should be CF. These CF groups are more favorably adsorbed on top-layer Ni sites (Ni*) directly bonded to –OH groups, as indicated by the minimum energy structures calculated for the NiO(CF) and NiOFr(CF) models (Fig. 10a and b, respectively). As can be observed, in both cases CF binding on Ni* cations results in significant structural changes on NiO surface, in particular regarding the local environment of Ni* sites (see also S7 and Fig. S23a, SI). In particular, Ni* cations are up-shifted by ≈1 Å with respect to the other top-layer Ni atoms. As a result, Ni* are bonded to two nearest-neighbour O atoms, an effect slightly more pronounced in the NiO(CF) model, i.e. in the absence of Fr (Fig. 10a, S1c, and S21, SI). Hence, Ni* sites exhibit a nearly planar three-coordinated environment, suggesting that Ni*-CF moieties could be characterized by a high reactivity in the OER process. In addition, even top-layer reticular Fr – which replace surface O atoms – are up-shifted by 1.2 Å with respect to top-layer oxygen (Fig. 10b), indicating that they could be prone to contact with incoming reactants.
To elucidate the role of Ni*CF and Fr defects in electrocatalysis, the electronic structures of NiO(CF) and NiOFr(CF) models were analyzed by calculating the corresponding density of states (DOS, Fig. 10c and d), and the projected DOS (pDOS, Fig. 10e and f). Remarkably, CF presence yields the appearance of a high density of empty states above the Fermi level at 1.32 eV and 0.98 eV for NiO(CF) and NiOFr(CF), respectively (Fig. 10c and d). Indeed, the formation of these new, easily accessible empty electronic states – absent for the pristine NiO surface (Fig. S23b, SI) - might be the atomistic origin of OER activity for the present electrocatalysts, since they could accept electron density from incoming OH− anions. A careful pDOS inspection reveals that these states are mainly localized not only on the Ni*-CF moiety, but also on the nearest-neighbour O atoms – i.e., on the local environment of the Ni* site (Fig. 10e and f). Notably, the density of such empty states is significantly higher for NiO(CF) than for NiOFr(CF), indicating that NiO surfaces with adsorbed CF moieties might be more efficient OER catalysts in comparison to the ones featuring both surface-adsorbed CF and F incorporation into NiO lattice. Conversely, the presence of reticular F is associated to the formation of new occupied states immediately below the Fermi level, essentially localized on Fr 2p-states (Fig. 10d and f), and does not generate new low-energy empty states, which would favourably boost the OER process.
Additional details on material preparation, characterization, and modeling are reported in the SI.
The data supporting this article are included as part of the SI.
| This journal is © The Royal Society of Chemistry 2025 |