Pan
Wang§
ab,
Ruqiang
Lu§
a,
Arthur
France-Lanord
c,
Yanming
Wang
c,
Jingjing
Zhou
b,
Jeffrey C.
Grossman
*c and
Timothy M.
Swager
*a
aDepartment of Chemistry, Massachusetts Institute of Technology, Massachusetts 02139, USA. E-mail: tswager@mit.edu
bSchool of Science, Westlake University, Hangzhou 310024, Zhejiang Province, China
cDepartment of Materials Science and Engineering, Massachusetts Institute of Technology, Massachusetts 02139, USA. E-mail: jcg@mit.edu
First published on 19th November 2020
Nanoscopic macrocycles could have unusual magnetic, optical, and electronic properties when compared to their linear counterparts. Conjugated π-systems in unsaturated macrocycles are particularly interesting as they have no end groups that limit electronic delocalization in equivalent linear oligomers. The rigid four-membered ring structure in 3,4-bis(methylene)cyclobutene with vicinal connections provides a vertex with an angle slightly less than 90°, which promotes macrocycle formation. We report herein a facile high-yielding synthesis of a series of 3,4-bis(methylene)cyclobutene-base π-conjugation macrocycles. The structure–property studies reveal that the smaller macrocycles are rigid crystalline frameworks and display symmetrical conformations in solution. The electrochemical, photophysical and magnetic properties of these macrocycles were also studied with a framework of characterization methods, revealing their size- and linkage-dependent properties. Density functional theory (DFT) calculations and molecular dynamics (MD) simulations at the molecular level suggest that several possible configurations are possible for macrocycles with larger ring sizes.
As a highly strained and air-sensitive isomer of benzene, 3,4-bis(methylene)cyclobutene has drawn much attention since it was first synthesized in the 1960s.20 The air-stable analogues were developed by Toda et al., by the thermal conversion of diallenes in the crystalline state.21–23 The introduction of aromatic substituents on the exocyclic methylenes and electron-withdrawing groups into the cyclobutene skeleton provides improved stability. Four-membered ring compounds that contain a bis(methylene)cyclobutene base structure have been extensively studied,23–26 and we have been interested to extend this unique structure as a vertex in macrocyclic compounds with different conjugation linkages to produce a series of fully conjugated macrocycles with persistent defined shapes.
Herein, we report the efficient template-free synthesis of a series of cyclobutene-based π-conjugation macrocycles with different ring sizes in high yields benefiting from the 3,4-bis(methylene)cyclobutene core structure bearing angular orientations less than 90°. Two-dimensional nuclear magnetic resonance (2D) NMR and variable temperature (VT)-NMR analysis demonstrated that these macrocycles are highly symmetrical in solution and single crystal X-ray crystallography revealed the packing mode and the planarity of the main-chain carbon atoms. The synthesized macrocycles can be chemically oxidized and the formation of radical cations (that can provide polarons in the solid state) was monitored by electron paramagnetic resonance (EPR) spectroscopy. SEM images revealed the relatively rigid crystalline macrocyclic framework. The optical and electrochemical properties were investigated, revealing the size- and linkage-dependent properties of these macrocycles (Fig. 1).
We synthesized 1,2-dibromo-3,4-bis(diphenylmethylene)cyclobutene 1via a three-step synthetic route as shown in Scheme 1. Glaser-Hay oxidative coupling reaction of the corresponding terminal alkyne 4 gave compound 3 in 89% yield. Following Toda's synthetic method,22 upon treatment of 3 with hydrobromic acid in acetic acid provided the brominated products 2 as a mixture. Thermal rearrangement in refluxing toluene afforded pure cyclobutene 1 in quantitative yield within 1 h. We explored cyclization reactions using Stille-coupling of cyclobutene 1 with 5,5′-bis(trimethylstannyl)-2,2′-bithiophene (2THSn). As shown in Table 1, using [Pd(π-cinnamyl)Cl]2 as the precatalyst and tBuXPhos as the ligand, the Stille-coupling reaction in toluene after 24 h gave a 34% yield of soluble red solids and side products that are not soluble in common organic solvents (Table 1, entry 1). MALDI-TOF mass spectrometry analysis reveals that the soluble portion are primarily macrocycles with 3 repeating units. Changing the ligand from tBuXPhos to XPhos increased the yield of the soluble portion to 43% (Table 1, entry 2). Microwave reaction conditions with a shortened reaction time to 4 h, increased the yield of soluble products to 83% (Table 1, entry 3). The MALDI-TOF mass spectrum analysis of macrocycle mixtures indicate the presence of four different ring-size macrocycles, namely the 3-mer A1, 4-mer A2, 5-mer A3 and a trace of the 6-mer A4 (From MALDI-TOF mass spectrometry: A1 (m/z = 1632.223, n = 3), A2 (m/z = 2176.527, n = 4), A3 (m/z = 2720.659, n = 5), A4 (m/z =3265.815, n = 6). The observed isotope distributions of all the different ring-size macrocycles from MALDI-TOF mass spectrometry are in agreement with the calculated values.
Entrya | Ligand | Yieldb (%) | MALDI-TOFc |
---|---|---|---|
a Reaction conditions: 0.15 mmol scale, 0.05 M, under N2 atmosphere. b Yield of the soluble mixture of macrocycle portion. Macrocycles were purified by passing through a pad of Celite and precipitated from MeOH. c 2-[(2E)-3-(4-tert-Butylphenyl)-2-methylprop-2-enylidene]malononitrile (DCTB) was used as the matrix in MALDI-TOF mass spectrometry with a PEG3000 calibration standard. d The reaction was carried out in a microwave reactor at 110 °C for 4 h. | |||
1 | t BuXPhos | 37 | 3-mer and other pieces |
2 | XPhos | 43 | 3-, 4-, 5-, 6-mers |
3d | XPhos | 83 | 3-, 4-, 5-, 6-mers |
The relative constitutions of macrocycles A1, A2 and A3 were quantified and isolated using high-performance liquid chromatography (HPLC) analysis (Fig. 2c). A4 was present only in trace quantities and wasn’t studied in detail. UV-vis spectroscopic analysis (Fig. 2d) shows that A1 has the maximum absorption band at 426 nm, whereas A2 is red shifted to 440 nm as a result of its longer effective conjugation length. A3 shows an absorption band at 427 nm similar with A1, suggesting a twisted configuration of the larger ring. Our observations suggest that there is no full delocalization of the whole π-system as the ring size increases, thus limiting the conjugation length in the ring. The molar absorption coefficients of the three macrocycles are around 7.0 × 104 M−1 cm−1 to 8.2 × 104 M−1 cm−1 at 427 nm, and the relative concentrations in the soluble reaction products were roughly estimated based on the integrated peak areas from HPLC analysis. As can be seen in Fig. 2c, the HPLC trace area with monitoring at 430 nm indicates the relative percentages of A1, A2, A3 to be 55.2%, 26.4% and 18.4% respectively. All of the macrocycles are emissive when dissolved in tetrahydrofuran (THF) and show a similar emission profile around 630 nm (Fig. 2e and f).
1H NMR spectra of the three isolated macrocycles A1–A3 indicate these macrocycles are highly symmetric in solution that only one set of proton signals of the repeating unit was observed. The combined information from 2D NMR heteronuclear single quantum coherence (HSQC) and heteronuclear multiple bond correlation (HMBC) analysis, allows for the assignment of all the proton signals (Fig. S1–S3, ESI‡). The protons on thiophene ring display different chemical shifts for each ring-size macrocycle (Fig. 3). For example, as shown for A1, the proton Ha, which is the closest to the cyclobutene ring, is shielded with a chemical shift at 5.67 ppm, whereas the proton Hb is de-shielded and resonates at 6.58 ppm. The different chemical shifts of the different ring-size macrocycles are indicative of the differences in their electronic and conformational structures.
Fig. 3 Structural elucidation of Macrocycles A1, A2 and A3 by NMR spectroscopy. (a) 2D NMR HMBC (500 MHz, 25 °C, THF-d8) spectrum of A1. (b) 1H NMR (500 MHz, 25 °C, THF-d8) spectra of A1, A2 and A3. |
Macrocycle A1 crystallizes more readily than the other macrocycles and displays interesting self-assembled morphologies when grown from different solvents.28 As visualized by scanning electron microscopy (SEM), crystals of A1 tend to form cylinders in various diameters when grown in chlorobenzene (Fig. 4d) and form fibrous structures when grown in THF (Fig. 4e). These fibrils have a smaller diameter that assemble into balls.
Macrocyclesa | Yieldb (%) | Tdc (°C) | λ abs(max) solutiond (nm) | λ em(max) emissione (nm) | λ abs(max) filmf (nm) | Quantum yieldg (%) |
---|---|---|---|---|---|---|
a Standard reaction conditions: 0.15 mmol scale, 0.05 M, under N2 atmosphere. b Yield of the soluble products. The macrocycles were purified by passing through a pad of Celite and precipitated from MeOH. c Initial decomposition temperature, onset temperature in TGA analysis. TGA analysis was conducted in N2 atmosphere with a ramping rate 20 °C min−1 to 900 °C. d In THF solution. e The excitation is at the maximum absorption wavelength. f Spin-coated films on glass slides with macrocycles dissolved in THF solution. g Quantum yields were measured in THF solutions with 1,4-bis(5-phenyloxazole-2-yl)benzene (POPOP) as the standard. | ||||||
A | 83 | 374 | 422 | 628 | 445 | 5.9 |
B | 76 | 339 | 352 | 688 | 380 | 6.5 |
C | 92 | 328 | 387 | 660 | 383 | 7.6 |
D | 99 | 339 | 440 | 603 | 440 | 7.3 |
As summarized in Table 1, thermal gravimetric analysis (TGA) reveals that the macrocycles display high thermal stability with initial decomposition temperatures ranging from 328–374 °C (Fig. S9, ESI‡). Differential scanning calorimetry (DSC) analysis of the macrocycle mixtures shows no obvious thermal transitions between 100 °C to 350 °C as expected as a result of the mixture of macrocycles and conformations, thereof appears to produce an amorphous state.
The macrocycle mixtures show different UV-vis absorption behaviors, which are related to their effective conjugation lengths (Fig. S8, ESI‡) and modest emissive quantum yields ranging from 5.9% to 7.6%. Macrocycles with three repeating units have been separated successfully by HPLC prep-column, giving macrocycle A1 (3 repeating units), B1 (3 repeating units), C1(3 repeating units) and D1 (3 repeating units) as single pure products. Their UV-vis and emission spectra were also studied in THF solutions. As shown in Fig. 5, D1 with a terthiophene linker has the longest conjugation length with absorption and emission maximum at λabs(max) of 440 nm and λem(max) of 615 nm respectively, while A1 displays a λabs(max) of 426 nm and a λem(max) of 634 nm. C1 displays two absorption bands at 319 nm and 397 nm, and its emission spectrum shows a λem(max) of 634 nm and a shoulder peak at 658 nm that are related to the absorption and emission of two different transition states. Similarly, B1 presents two absorption bands at 365 nm and 428 nm, and a broad emission band around 637 nm. The difference in conjugation lengths observed in these macrocycles with the same repeating units (three repeating units) could be attributed to the effective conjugation between the cyclobutene monomer and the different linkers. The conformations between the linkers and the cyclobutenes may vary and therefore affect the conformations in macrocycles. Based on the trends in the λmax values, it appears that the length of the linking heterocycles dominates the conformation structures: the terthiophene linker in D1 having the longest conjugation length and the single thiophene of B1 having the lowest degree of conjugation.
The synthesized macrocycles readily absorb I2 to create “doped” samples. Thin films were prepared by spin coating with macrocycles in THF solution (5 mg mL−1, 1500 rpm) and were then exposed to iodine vapor in a sealed chamber for 60 h at room temperature. After doping, the λabs(max) of the thin film of macrocycles mixtures A shifts from 445 nm to 395 nm, and a new strong absorption band arises at 793 nm that is related to the absorption band of polaronic or bipolaronic states of the macrocycles29 (Fig. 6a). The iodine treated samples also display an induced electron paramagnetic resonance (EPR) signal in solution phase (Fig. 6b). Upon adding excess amount of iodine to the dry toluene solution of macrocycle A1, a broad EPR spectrum was observed with a g-value of 2.0089, indicating the formation of polarons that have localized spin distribution in the macrocycles.30,31 Its spin intensity decreased over time, as the solution undergoes to higher doping levels, creating bipolaronic states (with charges of +4e and +6e) which are spinless.
To further study the redox behavior of these macrocycles, cyclic voltammetry (CV) was conducted on the macrocycle mixtures. A model compound RP1 with two single thiophenes attached to the cyclobutene was synthesized by Suzuki coupling reaction. The CV of RP1 dissolved in dichloromethane (DCM) solution produced that one quasi-reversible redox wave at E1/2 = 0.48 V (vs. Fc/Fc+) (Fig. S10a, ESI‡). The CV of macrocycles A1 spin-coated on the indium tin oxide (ITO) glass displays a single redox wave at E1/2 = 0.40 V (vs. Fc/Fc+) similar to RP1 (Fig. S10b, ESI‡). The CVs of the macrocycle mixtures of A, B, C and D were also studied as thin films on ITO glass and all had quasi-reversible redox waves at slightly lower potentials and thereby establishing the semi-conductive potential of these materials (Fig. S10c, ESI‡).
The DFT results are presented in Fig. 7. The structure of the A1 macrocycle differs slightly from the crystal structure, and the computed structure has all thiophene rings oriented towards the center of the molecule. This is not the case for all macrocycles and in D1 the thiophene units show alternating orientations. The macrocycles all share two main geometrical features: (1) the inner phenyl rings stack face-to-face with π–π interactions, and (2) the triangular ring formed by the thiophene groups is corrugated. Computed structures reveal similar orientations of the outer phenyl groups of the X-ray crystal structure. Both the HOMO and LUMO orbitals of the macrocycles are significantly delocalized throughout the π-conjugated network for all macrocycles. Finally, the calculated HOMO–LUMO gaps of the A1, B1, C1, and D1 molecules are 2.40, 2.57, 2.54, and 2.42 eV, respectively. It is important to note that the calculated HOMO–LUMO gap is the difference between the vertical ionization potential and the vertical electron affinity, which is typically larger than the actual band gap in the condensed phase as a result of interactions between π-conjugated molecules.37 The DFT calculations are in agreement with the experimental observation of these macrocycles. MD simulations for larger macrocycles were also performed at the molecular level in the gas phase, which suggest a few possible configurations of the isolated macrocycles exist at room temperature (300 K). Here the calculated configurations for macrocycles with higher repeating units (n > 3) demonstrated a tendency to buckle and fold (Fig. S14, ESI‡).
Footnotes |
† Dedication: To the inspiring example of Fred Wudl and his many pioneering contributions in the design, synthesis and study of organic electronic materials. |
‡ Electronic supplementary information (ESI) available. CCDC 2011836. For ESI and crystallographic data in CIF or other electronic format see DOI: 10.1039/d0qm00824a |
§ P. W. and R. L. contributed equally. |