Department of Chemistry, Northwestern University, Evanston, IL 60208, USA. E-mail: jkalow@northwestern.edu
First published on 8th April 2020
Vitrimers are a class of covalent adaptable networks (CANs) that undergo topology reconfiguration via associative exchange reactions, enabling reprocessing at elevated temperatures. Here, we show that cross-linker reactivity represents an additional design parameter to tune stress relaxation rates in vitrimers. Guided by calculated activation barriers, we prepared a series of cross-linkers with varying reactivity for the conjugate addition—elimination of thiols in a PDMS vitrimer. Surprisingly, despite a wide range of stress relaxation rates, we observe that the flow activation energy of the bulk material is independent of the cross-linker structure. Superposition of storage and loss moduli from frequency sweeps can be performed for different cross-linkers, indicating the same exchange mechanism. We show that we can mix different cross-linkers in a single material in order to further modulate the stress relaxation behavior.
A more recently reported class of CANs that exchange by associative mechanisms, known as vitrimers,15–18 retain a cross-linked structure during swelling and heating, but can still be remolded and repaired.5 Overall cross-link density is conserved since bond breakage only occurs after another covalent bond has been formed; these materials are expected to maintain a constant rubbery plateau modulus during topological rearrangement.2 A wide array of associative dynamic covalent chemistries have been employed in vitrimers, including transesterification,19–21 olefin metathesis,22,23 dioxaborolane exchange,24–26 silyl ether exchange,27 and several others.28–37 Surprisingly, despite the number of reactions studied, there are no systematic studies that examine the effect of the cross-linker structure on vitrimer properties. In this paper, we show that small structural modifications to cross-links in a vitrimer can offer control over stress relaxation over a wide range, without affecting the stiffness or flow activation energy of the materials.
Strategies to control the rate of vitrimer flow primarily rely on the effect of catalysts38,39 and cross-link density,31,40–42 with isolated examples examining macromolecular architecture43 and strand flexibility.44 In a pioneering study, Leibler and co-workers demonstrated that changing the catalyst type and concentration affects flow activation energies for ester-based vitrimers.45 Bates and co-workers later identified a surprising inverse relationship between the pKa of Brønsted acid catalysts and flow activation energy.46
Catalysts can suffer from leaching and deactivation, motivating our interest in catalyst-free exchange reactions for vitrimers. We previously demonstrated that the conjugate addition–elimination of thiols to a Meldrum's acid-derived acceptor47 in a PDMS vitrimer enables at least ten reprocessing cycles without loss of properties (Scheme 1).48 Here, we synthesize a series of conjugate acceptor cross-linkers and compare their reactivity in vitrimers. Key differences in reactivity can be rationalized based on calculated transition states. We obtain vitrimers exhibiting a wide range of stress relaxation times, spanning over 4 orders of magnitude, with nearly identical stiffnesses. We can superimpose frequency sweeps for three distinct cross-linkers with a horizontal shift factor, suggesting that relaxation occurs through a common mechanism. Finally, we can further tune the stress relaxation profiles by mixing cross-linkers with different reactivities into single networks. This study revealed two new cross-linkers that enable significantly faster stress relaxation compared to the original Meldrum's acid-derived acceptor.
![]() | ||
Scheme 1 Mechanism of the conjugate addition–elimination exchange reactions in the elastomeric PDMS vitrimer studied here. |
![]() | ||
Fig. 1 (a) General synthesis for cross-linkers used in the study. (b) Structures of different cross-linkers used in the study. |
Tetrahedral intermediates for the acyclic cross-linkers DP and CN orient the proton away from the thiols, and correspondingly, no closed transition states were located. The Nsp lone pairs on each nitrile of CN point away from the site of nucleophilic attack. The bond rotations required in DP to accommodate a cyclic transition state would likely result in unfavourable steric interactions (Fig. S15–S17†). Thus, the acyclic cross-linkers lack an internal base to accelerate the exchange process.
To compare the effect of cross-linker structure in vitrimers, stress relaxation experiments were performed using shear rheology (Fig. 3a; for additional details, see ESI†). The vitrimer networks are named based on the cross-linker used (e.g., CY-Net). The rate of the relaxation process can be characterized with respect to a characteristic relaxation time constant, τ*. Assuming Maxwell behaviour, τ* is defined as the time needed for the relaxation modulus to decrease to 1/e of its initial value. The τ* values for this series of cross-linkers span 4 orders of magnitude, following the trend CY < BA < IND ∼ MA ≪ CN ∼ DP (Fig. 3b). This trend is consistent with the calculated ΔG‡ values, suggesting that the stress relaxation in these materials is directly correlated to the exchange kinetics. The wide range in stress relaxation rates was accompanied by modest differences in stiffness. The rubbery plateau moduli of these networks at 150 °C were determined by frequency sweeps between 100 and 1 rad s−1 and were found to be similar for all cross-linkers, ranging between 100 and 130 kPa (Fig. 3b). The similarity of the plateau moduli and gel fraction studies (Table S10†) suggest that cross-link density is not affected by the structure of the cross-linker, consistent with an associative mechanism.
![]() | ||
Fig. 3 Mechanical properties of the networks. (a) Representative normalized stress relaxation profiles at 150 °C. (b) Calculated τ* values for the different cross-linked vitrimers (bar graph, left axis) and their rubbery plateau moduli at the same temperature (circle symbols, right axis). Error bars are based on student's t distribution. The τ* values were calculated using 1/e of the relaxation modulus for the cyclic cross-linkers and by extrapolating a stretched exponential function for the acyclic cross-linkers (see ESI for more detail†). (c) Arrhenius plots for stress relaxation of networks derived from the cyclic cross-linkers. (d) Calculated flow activation energies for the networks. Error bars are based on the error analysis of the fitted slopes. |
The flow activation energy (Ea) is determined by measuring τ* as a function of temperature based on the Arrhenius relationship (eqn (1)):
![]() | (1) |
Surprisingly, the flow activation energies calculated for the different cyclic cross-linkers were within experimental error, with their averages ranging between 60 and 68 kJ mol−1 (Fig. 3c and 3d). While this result differs from the calculated ΔG‡ values, for multistep reactions, Eyring ΔG‡ values are not equivalent to Arrhenius activation energies (Ea). Instead, the difference in relaxation times is driven by the pre-exponential factor, τ0, represented by the change in y-intercept (Table S11†). τ0 has been defined as the relaxation time at infinite temperature, but the physical underpinnings of this value in vitrimers are not well understood.5 For the acyclic cross-linkers, the experimentally accessible temperature range was too narrow for an accurate Arrhenius analysis.
Activation energy values represent the temperature sensitivity of a process, and not the absolute kinetics. Rational strategies to tune the flow activation energy, Ea, and the pre-exponential factor, τ0, are necessary to guide optimization of vitrimer properties. For example, to minimize creep at service temperatures but enable flow at elevated temperatures without decomposition, high Ea is desirable.28 In ester and vinylogous urethane vitrimers, catalysts modulate relaxation times by changing both Ea and τ0.27,28,43 Our results show that the absolute rate of stress relaxation can be modulated without affecting the temperature dependence by changing the structure of the cross-linker. It should be noted, however, that the flow activation of the polymer can differ from the small molecule activation energies.5,49
Some vitrimer systems exhibit a change in exchange mechanism as a function of temperature or additives.50,51 We sought to confirm that changing the structure of the cross-linker in the vitrimer did not influence the mechanism of exchange. Typically, time–temperature superpositions (TTS) of frequency sweeps are used in polymer rheology to determine if the relaxation processes scale as a function of temperature. In order to determine if the relaxation processes in our vitrimers scale as a function of cross-linker reactivity, a time–cross-linker superposition (TCLS) was constructed at 150 °C (3% strain, 0.01–100 rad s−1) for representative cross-linkers (Fig. 4). This type of analysis has been performed by researchers in dissociative systems where the shift factor of the superposition can relate to the kinetics or activation energy of cross-linker dissociation.6,7 The networks in this study contained 1.25 mol% of the cross-linker, which allowed access to the terminal regime. We were able to superimpose the CY-Net and BA-Net storage (G′) and loss (G′′) moduli curves onto the reference IND-Net data using only horizontal shift factors. This superposition suggests that the mechanism of stress relaxation is indeed identical for the cyclic cross-linkers; the only difference between samples is how fast or slow the collective relaxation process is.
![]() | ||
Fig. 4 Time—cross-linker superposition for both the storage (G′) and loss (G′′) moduli of networks with three different cross-linkers (IND, BA, and CY). IND was used as the reference. |
The horizontal shift factors (αT) were calculated from the crossover frequencies (ωc), which are inversely related to the characteristic stress relaxation times τ* for an ideal Maxwell material (eqn (2)).
![]() | (2) |
Furthermore, a vertical shift factor was not required, and the rubbery plateau moduli of the samples with 1.25 mol% cross-linker ranged between 8 and 11 kPa, again demonstrating that an associative exchange mechanism can decouple stiffness and stress relaxation.
For dissociative reversible networks, mixing cross-linkers with the same exchange mechanism but different relaxation rates modulates stress relaxation profiles.15,52,53 While Dichtel,54 Chen,55 and Guo56 have mixed associative and dissociative cross-links in a single network, we are interested in the effect of mixing mechanistically similar, kinetically distinct associative cross-links. We formulated three separate samples based on binary mixtures of cross-linkers (1 mol% each): CY/MA-Net, BA/MA-Net, and BA/DP-Net. Stress relaxation measurements were carried at 140 °C (Fig. 5). As expected based on the stress relaxation of the single cross-linker networks, the stress relaxation times follow the trend CY/MA-Net < BA/MA-Net < BA/DP-Net. Each stress relaxation profile is intermediate to those of its individual cross-linker counterparts (Fig. 5a through c).
![]() | ||
Fig. 5 Normalized stress relaxation data for (a) CY-Net, CY/MA-Net, and MA-Net; (b) BA-Net, BA/MA-Net, and MA-Net; (c) BA-Net, BA/DP-Net, and DP-Net at 140 °C. |
The shape of the normalized stress relaxation curves for the mixed systems indicate additional complexity. Surprisingly, the BA/MA-Net relaxation data could be fitted to an ideal Maxwell model with an activation energy similar to that of the individual cross-linkers (Fig. S13 and S14†), whereas CY/MA-Net and BA/DP-Net relaxation deviated from ideal Maxwell behaviour, suggesting that multiple relaxation modes are operative (Fig. S11 and S12†). We conclude that the presence of either a singular or multiple relaxation modes depends on the relative relaxation times for each individual cross-linker. If the relaxation times for the individual cross-linkers are within an order of magnitude, the mixed cross-linker system exhibits a single intermediate relaxation mode. When the individual relaxation rates differ by several orders of magnitude, we observe several distinct relaxation modes. This relaxation behaviour is more varied than what has been observed in dissociative systems: mixed boronic ester cross-links resulted in single unimodal Maxwell distributions,52 and mixed metal–ligand15 and protein–protein cross-links53 showed a distinct relaxation mode for each component. The relevance of the Maxwell model to vitrimers is under investigation in our lab.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0py00233j |