Minal
Wable
ab,
Batuhan
Bal
a and
Ömer Özgür
Capraz
*ab
aChemical Engineering, Oklahoma State University, Stillwater, OK 74078, USA. E-mail: capraz@umbc.edu
bChemical, Biochemical and Environmental Engineering, The University of Maryland – Baltimore County, Baltimore, MD 21250, USA
First published on 18th January 2024
Sodium chromium oxide, NaCrO2, exhibits promising features as a cathode in Na-ion batteries, yet it encounters challenges with its capacity fading and poor cycle life. NaCrO2 undergoes multiple phase transitions during Na-ion intercalation, eventually leading to chemical instabilities and mechanical deformations. Here, we employed the digital image correlation (DIC) technique to probe electrochemical strain generation in the cathode during cycling via cyclic voltammetry and galvanostatic cycling. The electrode undergoes significant irreversible mechanical deformations in the initial cycle, and irreversibility decreases in the subsequent cycles. During desodiation and sodiation, the electrode initially undergoes volume contraction at a lower state-of-(dis)charge followed by expansions at a higher state-of-(dis)charge. The similar progression between strain and capacitive derivatives points out the phase-transition-induced deformations in the electrode. The evolution of cumulative irreversible strains with cycling time indicates the irreversibility rising from the formation of cathode-electrolyte interphase layers. The study demonstrates valuable insights into mechanical deformations in NaCrO2 electrodes during battery cycling, which is critical to engineer mechanically robust cathodes for Na-ion batteries.
NaCrO2 is one of the promising candidates for practical application in SIBs due to its flat and smooth voltage plateau. This voltage behavior shows similarity with the ones observed in widely commercialized LiCoO2 cathodes in LIBs. Additionally, it offers high thermal stability, wide temperature adaptability, and remarkable rate capability achieved through carbon-coating, with minimal side reactions and high coulombic efficiency.13–16 NaCrO2 delivers a limited reversible capacity of about 120 mA h g−1, with only approximately 0.5 Na extraction possible in NaCrO2, and suffers from rapid capacity fading during cycling.7,17 Previous studies show that NaCrO2 undergoes multiple phase transitions during cycling, which have been investigated through ex situ X-ray diffraction (XRD), synchrotron-based XRD, in situ X-ray absorption spectroscopy (XAS) and electron paramagnetic resonance (EPR) spectroscopy.17–19Operando atomic force microscopy provided a correlation between electrochemical redox reactions and nanoscale deformations in the electrode structure.20–22 However, overall mechanical deformations and their relationship with phase transition during Na-ion intercalation in NaCrO2 are not well known.
The phase transition in the electrode during intercalation leads to mechanical deformations, which impacts the electrochemical performance of battery materials.23 Repeated ion intercalation causes continuous volumetric expansions/shrinkage and associated strain generation in the electrodes. Various techniques have investigated mechanical deformations in batteries, including curvature measurement, Digital Image Correlation (DIC), and nanoindentation.24–26 Overall, these studies provided crucial information about governing factors behind reversible and irreversible deformations in the electrode. Curvature measurements in LiMn2O4, coupled with XRD analysis, indicated the generation of irreversible stress beyond 4.05 V during the first cycle, and it was associated with the formation of oxygen vacancies and crystallinity loss.24 Digital image correlation analysis on graphite electrodes in Li-ion batteries categorized strains as induced reversible deformations induced by phase-transition and irreversible strains due to the formation of solid–electrolyte interphase (SEI).27 Furthermore, the evaluation of mechanical properties of SEI on both lithium and lithium-free anodes and its impact on cycling performance has been investigated through rapid nanoindentation analysis.28 The combination of DIC and X-ray photoelectron spectroscopy (XPS) study elucidated the formation of the cathode-electrolyte interphase (CEI) layers on LiFePO4 cathodes during the early cycles and its impact on irreversible mechanical deformations.25 Synchronization of stress and strain measurements differentiate the impact of the surface resistance versus structural deformations in the battery electrodes.29,30 Probing strains in the cathodes also provided information about the reversible deformations in the electrode structure associated with the redox reactions.29,30
This study aims to probe electrochemical strains in NaCrO2 cathode during cycling using the DIC and electrochemical methods. The electrode was sodiated/desodiated via both cyclic voltammetry and galvanostatic cycling while probing strain generation in the electrode. The strain behavior showed similarity when the electrode was cycled with either cyclic voltammetry or galvanostatic cycling. Significantly large irreversible strains were recorded in the initial cycle, and irreversibility decreased in the subsequent cycles. The strain generation during desodiation substantially reduced with the cycle number. Overall, the electrode initially undergoes volume contraction, followed by expansion during each sodiation and desodiation cycle. Strain derivatives were calculated to further investigate the relationship between reversible deformations and phase transition in the electrode. The cumulative irreversible strains increased linearly with the square root of cycling time, where the slope was found to be similar to our previous work on NaFePO4 cycled under similar electrochemical conditions. This correlation points out a formation of the CEI-induced irreversible deformations in the electrode.
The associated strain generation in NaCrO2 is shown in Fig. 2b. The positive and negative strain changes imply expansion and contraction in the electrode volume, respectively. In the first desodiation process, the electrode initially experienced −0.05% negative strains, followed by an increase of about 0.51% by the end of the first desodiation. During the first sodiation, there was a generation of −0.11% negative strains followed by a generation of 0.01% positive strains, and the cumulative strains became 0.52% by the end of the first cycle. The irreversible strain generation progressively slowed down in the later cycles and became 1.19% at the end of the fifth cycle. To provide a better picture, current evolution, and strain change during the third cycle are plotted in Fig. 2c and d. There are negligible deformations during the early stages of the third cycle desodiation until the voltage reaches 2.85 V. Then, the electrode began to contract at the onset of the current rise at 2.85 V, and −0.11% negative strains were generated until 3.1 V, where the current reached its peak. At higher voltages, the electrode experienced a positive strain generation of about 0.08% until the end of the third desodiation. The electrode underwent negligible deformation during the early stages of the third sodiation until 3.01 V. Then, the electrode experienced a negative strain generation (about 0.06%) between 3.01 and 2.87 V, followed by expansions of about 0.16% between 2.87 V and 2.69 V. At the lower voltages, there is a negligible deformation in the electrode until the end of the third cycle. Similar mechanical deformations behavior is observed in the subsequent desodiation and sodiation cycles (Fig. S5, ESI†).
NaCrO2 cathode was sodiated/desodiated via galvanostatic cycling to further investigate the mechanical deformations in the electrode (Fig. 3 and Fig. S6, ESI†). The galvanostatic cycle allows the control reaction rate at the surface of the electrode. We chose to cycle the battery at C/25 because it takes about the same time when cycling via CV at 50 μV s−1. There is a voltage plateau at around 3.0 and 2.9 V during desodiation and sodiation, respectively.
Previous ex situ XRD studies observed O3R and O3R + O3M phases during the voltage plateau.17 Multiple shorter plateaus were recorded at the higher potentials associated with the phase changes, O3R + O3M ↔ O3M ↔ O3M + P3M ↔ P3M in the cathode.17 Desodiation and sodiation capacities in the first cycle were calculated as 93.8 mA h g−1 and 79.4 mA h g−1. The capacities became more reversible at later cycles. The desodiation and sodiation capacities in the 3rd cycle were 79.5 mA h g−1 and 76.0 mA h g−1, respectively. The theoretical capacity of the NaCrO2 electrode when discharged to Na0.5CrO2 is 125 mA h g−1. Since capacitates were slightly lower in strain measurements, we conducted additional measurements using a coin-cell configuration with a galvanostatic cycle at C/25. The capacity of the electrode was about 120 mA h g−1 in the coin cell experiments (Fig. S7, ESI†). Therefore, the experimental capacity of the NaCrO2 cathodes in our study is close to the theoretical capacity of the electrode. The slightly lower capacity in strain measurements is attributed to using much thicker electrodes in free-standing orientation in strain systems compared to coin-cell configurations.
The corresponding strain generation during a galvanostatic cycle is shown in Fig. 3b. During the first desodiation, a negligible strain was generated until capacity reached about 25 mA h g−1. Then, almost 0.3% strain was generated between a capacity of 25 to 70 mA h g−1, corresponding to a 3.0 V to 3.25 V voltage plateau. There is negligible strain generation at higher voltages (>3.25 V). The strain became 0.35% at the end of the first desodiation. During the first sodiation, the electrode initially contracted between 3.6 and 2.93 V, then expanded at a higher state of sodiation (2.92 to 2.3 V). The cumulative strains were about 0.43% at the end of the first cycle. The irreversible strain generation slowed down with further cycling, and it became 0.97% at the end of the fifth cycle. Interestingly, irreversible strain generation in the galvanostatic cycle (Fig. 3b) is very similar to the ones recorded during CV (Fig. 2b). There were similar irreversible strains in both cases after about 65 hours of electrochemical cycling by the end of the fifth cycle.
Beyond the first cycle, the mechanical deformations were very similar between each sodiation and desodiation. Strain change and voltage profiles for the third cycle were plotted in Fig. 3c and d for better visualization. At the initial period of desodiation, there is a negative strain generation of about −0.12%, which coincides with the first voltage plateau at around ∼3.0 V. In literature, the voltage plateau has been linked with the phase change from O3R → O3M.18
According to the previous XRD studies, c-axis lattice parameter increases due to increasing interslab distance between CrO2 layers while a- and b-lattice parameters decrease due to shrinkage between the Cr–Cr distance. They attributed the continuous increase in c-axis to the increased repulsion between CrO2 slabs and the continuous decrease in a- and b-lattice axis to the increasing oxidation state of the Cr as more Na is extracted.18 The XANES spectra demonstrated an unexpected behavior in Na–Cr bond length, which contracts in a- and b-axis while expanding in c-axis during desodation.18 Strain measurement in our study is sensitive to volumetric changes in the composite electrode due to lattice volume change upon Na-ion intercalation; therefore, it does not provide directional changes in the lattice slabs. Since the electrode underwent contractions in our measurements, we propose that a decrease in Cr–Cr distance dominates the deformations leading to negative strains in the electrode during the initial desodiation period. At higher voltages (>3.0 V), the electrode experienced a positive strain generation (0.04%) until the end of desodiation. During this period, multiple shorter plateaus at the higher voltages and XRD analysis in the literature indicated the phase changes, O3M ↔ O3M + P3M ↔ P3M in the cathode.17 Interestingly, the slope of the positive strain changes during this period, indicating the fundamental difference in the crystal structure based on the phase changes. In this period, XRD studies in the literature reported increases in interslab distance between CrO2 layers while the Cr–Cr distance decreased.17,18 Since the composite electrode expanded during this period, the deformations in the lattice volume were dominated by increased interslab distance between CrO2 layers. During the initial period of the third sodiation, there was a negligible amount of strain generation in the electrode until voltages reached their first plateau. Then, the electrode experienced about −0.02% during the voltage plateau at 2.95 V. In the literature, the plateau has been associated with the phase changes from P3M → O3M.34 At higher sodiation capacity, the direction of the strains changed from negative to positive, and the electrode underwent 0.13% deformation during the second voltage plateau at 2.9 V. This is associated with phase changes from O3M → O3R in the literature.34
Overall, both galvanostatic and CV tests indicate that the electrode experiences contraction, followed by expansions during each desodiation and sodiation process. Strain generation in the electrode showed a strong correlation with the electrochemical behavior. It indicates the role of phase transition on the mechanical deformations in the electrode. In both tests, the electrode showed reversible and irreversible deformation. To better understand the mechanisms behind the reversibility, we conducted further analysis by calculating strain derivatives with potential and irreversible strain with time.
Fig. 4 Capacity derivatives (dQ/dV) and strain derivatives (dε/dV) during (a) and (c) desodiation and (b) and (d) sodiation process, respectively during galvanostatic cycling. |
Four distinct peaks are observed during desodiation, labeled with Roman letters i–iv, and three during sodiation, marked as v–vii in Fig. 4. The derivatives were calculated during sodiation when the voltage decreases, whereas during desodiation, the voltage increases. Therefore, minima in strain derivatives during sodiation indicate the onset of expansion, which correlates with the onset of contraction during desodiation. These capacity derivative peaks are associated with the redox reaction involving Cr+3/Cr+4, occurring within the potential range of 2.3 to 3.6 V.18 The peaks at different potentials were attributed to a sequence of phase transitions from O3R to O3M and then to P3M. The intensity of strain derivatives, as represented by the magnitude of the peak in the dε/dV vs. V plot. The evolution of strain derivatives hints at the structural changes in the electrode due to lattice mismatch between the Na-rich phases and the Na-poor phases in the electrode. The location of the minima/maxima of the strain derivatives aligns very well with the maxima during desodiation and minima during sodiation in the capacity derivatives with ± 0.02 V margin. This alignment indicates a correlation between redox reactions and structural changes in the lattice. The direction of the strain derivatives changes within the sodiation and desodiation cycles. This demonstrated the directional change in the mechanical deformations as lattice parameters were either contracted or expanded, depending on the phase transition. Strain peaks at i and vii are in negative directions, whereas all other strain peaks are positive. The directional patterns of the strain derivative peaks indicate the distinct difference in the deformations resulting from the phase transition between O3R ↔ O3R + O3M ↔ O3M ↔ O3M + P3M ↔ P3M. The variations in the lattice parameter have been studied using in situ XRD.18 The findings reveal that during the desodiation process, the lattice parameter ‘c’ is continuously increasing, whereas ‘a’ and ‘b’ are continuously decreasing. However, the study lacks information on the volumetric changes during cycling. Using the DIC technique, the intensity of strain derivatives gives the perspective about the extent of volume change during the phase transitions in the desodiation and sodiation process. During the desodiation process, the maximum intensity of dε/dV is also observed at ca. 2.97 V, relating to the peak intensity of dQ/dV (2.98 V). Similarly, during desodiation, the maximum peak intensity is observed at 2.93 V, relating to the peak intensity of dQ/dV (2.93 V). Overall, strain derivatives calculation provided insights into dynamic structural changes in the NaCrO2 cathodes during cycling.
It is important to address possible heterogeneity in the cathode during cycling. The ion intercalation may not occur at the same rate if there is a significant heterogeneity due to particle size differences at faster scan rates. A recent synchrotron nano-holotomography study demonstrated local network heterogeneity in composite NMC cathodes when cycled at 5C rates.38 We also presented the high heterogeneity in the composite lithium iron phosphate (LFP) cathodes when cycled at faster rates (e.g., 2.5C). The heterogeneity was suppressed in the LFP cathodes when cycled at much slower rates (e.g., C/25).39 Here, the composite NaCrO2 cathodes were cycled at a C/25 rate to avoid heterogeneity in the composite network during cycling. To further verify it, we compared horizontal normal exx, vertical normal eyy, and shear strains exy in the composite electrode during galvanostatic cycling at C/25 rate in Fig. S3 (ESI†). The evolution of exx and eyy normal strains are similar during the cycling, and there is a negligible amount of exy strains in the composite electrode. Therefore, Fig. S3 (ESI†) indicates that heterogeneity in the composite NaCrO2 cathode was minimal when cycled at C/25 in our study.
Fig. 5 Strain trends during desodiation, sodiation process and irreversible strain generation during (a) galvanostatic cycling and (b) cyclic voltammetry in each cycle; (c) cumulative irreversible strain evolution in NaCrO2 electrode plotted against the square root of cycle time. The original data is from Fig. 2, 3 and Fig. S8, S9 (ESI†). Trails 1 and 2 show the repeated experimental results performed under the same galvanostatic cycling and cyclic voltammetry for figure a and b, respectively. |
Delamination, swelling in the composite electrode, particle fracture, and the formation of cathode-electrolyte interphase (CEI) layers can lead to irreversible mechanical deformations in the electrode. Adhesion between the current collector and the composite electrode can be loosened upon repeated intercalation, leading to delamination in the composite electrode.40–43 In our study, we prepared free-standing composite electrodes for digital image correlation as described in the experimental part, and the electrode was tested only for the initial five cycles at a slow rate. Therefore, delamination is unlikely to be the factor behind the irreversible strains observed in our study. Swelling in the composite electrodes results from the interactions between electrolyte and polymer binders in the composite network. Organic electrolyte intake into the composite network leads to volumetric expansions in the electrode.44–46 Fig. S2 (ESI†) shows a negligible amount of volumetric expansions during the open circuit period before the electrochemical testing; therefore, swelling is unlikely to contribute to irreversible strains in Fig. 5.
The electrode experienced large irreversible strain by the end of the first cycle compared to the subsequent cycles. The deformation mechanisms are much more complicated due to the CIE layers and mechanical instabilities in the electrode during the first cycle. The combination of DIC with XPS demonstrated the generation of large irreversible positive strains in lithium iron phosphate cathodes when cycled in LiPF6-containing organic electrolytes. The irreversible strains were attributed to the formation of the CEI layers. Interestingly, when the electrode cycled in LiClO4 salt, the irreversibility in the first cycle was much smaller than in LiPF6–containing electrolyte.25 Iron phosphate cathode experienced tremendous strain generation in the first cycle upon Na intercalation, leading to irreversible deformations in the electrode.47 Particle fracture is also reported in Ni-rich cathodes for Li-ion batteries during the first cycle when cycled at high voltages.48
Beyond the first cycle, there is a linear relationship between cumulative irreversible strain generation and the square root of time (t0.5) in the NaCrO2 cathode in Fig. 5c, suggesting the irreversible strain generation due to CEI layer formation on the cathode. CEI layers typically originate from the degradation of electrolytes on the cathode electrode surface due to chemical reactions between electrolyte and electrode surface, generally at high voltages. It is well-documented in the literature about the correlation between the increase in the thickness of SEI on the anode or CEI layers on the cathode with the square root of time, t0.5.49,50
The average slope in Fig. 5c is about 0.133 ± 0.015 (% h−0.5). Interestingly, in our previous study,51 the slope for the NaFePO4 electrode was found to be 0.134 (% h−0.5). Both NaCrO2 cathodes in this study and NaFePO4 cathodes in the previous study were cycled at the same rate and same electrolyte solution (NaClO4 in EC: DMC). The similarity in irreversible strain slope between two different cathodes further indicates that the irreversible are associated with the cathode-electrolyte interphase (CEI) layer formation.
Footnote |
† Electronic supplementary information (ESI) available: Fig. S1: Experimental setup of custom battery cell for strain measurements, Fig. S2: Strains during open circuit period, Fig. S3: Comparison of normal and shear strains during cycling, Fig. S4: Galvanostatic charge–discharge profiles in coin cell testing, Fig. S5–S9: Strain evolution in the NaCrO2 at different cycle numbers cycled either with galvanostatic cycling or cyclic voltammetry. See DOI: https://doi.org/10.1039/d3ya00563a |
This journal is © The Royal Society of Chemistry 2024 |