Plastic, due to its low cost, light weight, and tunable mechanical strength, is one of the most commonly used materials in daily life. However, the massive production of plastics in the last century has resulted in an environmental crisis globally, clogging oceans and poisoning communities around the world. Furthermore, the traditional methods for handling plastic waste, such as incineration and landfill disposal, can easily result in the generation of excessive amounts of microplastics (MPs), which lead to severe environmental pollution and pose a great threat to living organisms. Photocatalytic conversion of plastics to light-weight hydrocarbons and recycling are considered to be promising strategies towards the mitigation of MPs and have attracted a great deal of attention in the last few decades. In this review, a few representative and frontier studies on photocatalysis are presented as green promising methods towards the degradation of (micro)plastics. Initially, we introduce the harmful nature of waste (micro)plastics and discuss the background of photocatalysis. Then, the mechanisms for the photocatalytic degradation of (micro)plastics are presented, followed by the classification of photocatalysts. Also, we highlight conventional inorganic semiconductor oxides (TiO2, ZnO, etc.) and organic–inorganic hybrid composites, including doped and surface-modified nanoparticles. To further improve the efficiency of photocatalytic degradation, several approaches related to reactants, photocatalysts, and reaction conditions are proposed. Finally, based on current photocatalyst-mediated (micro)plastic degradation techniques, we provide some existing limitations and a perspective towards future research directions. This review systematically summarizes the efforts devoted to the photocatalysis of plastic and progress made in the degradation rate.
Nowadays, the most common ways of handling plastics are landfill disposal, incineration and mechanical reprocessing (Fig. 1). Till 2015, the world has produced 6.3 billion tons of waste plastics in total, of which 12% was incinerated and 79% was landfilled or abandoned in the natural environment.7 It is also estimated that if this status is maintained, 12 billion tons of waste plastic will be buried, incinerated, or discarded into the natural environment.8 However, these methods are only transient, which cannot alleviate the environmental problems caused by plastics permanently. Furthermore, the abuse of these strategies can lead to severe environmental issues. Among them, plastic landfills need large area of lands and can cause chronic pollution with nearly zero payback;9 the incineration of plastics causes poisonous gas emissions and deleterious chemical compositions such as CO, furans, dioxins and volatile organic compounds;10 and even worse, mechanical reprocessing requires presorting and damages their mechanical performances.11 All these physical methods have no significant effects on reducing the amount of castoff plastics and can inversely cause more severe environmental problems with the generation of microplastics. To date, microplastics have been found in seawater, seafloor sediment and even in human blood and lungs, which is much more dangerous than the influence caused by common plastic wastes.12
Compared to the typical ways of managing waste plastics, innovative chemical techniques for the degradation of plastics are emerging, which are more environmentally friendly, productive, and can even convert plastics into value-added products (Fig. 1),13 including biochemical conversion, microwave-assisted conversion, plasma-assisted conversion, supercritical water conversion, compatibilization, pyrolysis, gasification, polymer design and modification, and photoreforming.14 In addition to their environmentally friendly nature, these approaches are similar, exhibiting advantages and disadvantages. On the one hand, they can decrease the time for plastics to decompose, which takes hundreds of years employing traditional methods, while that for emerging strategies is a few days and even a few hours.15 Also, during the degradation processes, clean energy and high-value-added products are produced, contributing to the achievements of superior commercial benefits.16 On the other hand, the shortcomings of these approaches are also prominent due to their low yielding rate and significant cost.17 Although chemical disposal methods can avoid the production of detrimental substances to a large extent, they lack product regulation and have an extremely low energy efficiency.18,19 Besides, presorting is required in most strategies, further raising the cost of investments.15 Also, although quality corrosion and recovery loss are largely avoided compared with conventional methods,20 these drawbacks greatly hinder their promotion. To achieve the large-scale decomposition of plastic wastes, improving the chemical recycling and upcycling of (micro)plastics are necessary and researchers have been devoted to eliminating the above-mentioned limitations. Among the novel chemical methods for the degradation of plastics, photocatalysis is a superior method to overcome these defects. Thus far, many studies have elaborated the many strengths of photocatalysis in decomposing (micro)plastics as a rapid and stable technique with a relatively high efficiency.21
In contrast to other thermochemical and biochemical routes, which may require high energy consumption and harsh reaction conditions such as extremely high temperature and pressure, photocatalysis is comparatively greener and cheaper owning to its suitable energy input and moderate reaction conditions applying sunlight or UV light as the energy source under ambient temperature and pressure.22 Photocatalysis has a promising outlook in environmental protection due to its redox property,23 which is related to the excitation of valence electrons to the conduction band and the valence band holes can work as oxidizing agents.24 Generally, photocatalysis is carried out in cooperation with several steps of hydrogen evolution reaction and oxygen evolution reaction,25 finally generating H2O, CO2 and other value-added chemical products such as H2 and low-molecular weight organic matter.13 TiO2 is the earliest photocatalyst, which was first reported in 1974,26 with a comprehensive review on the degradation of polyolefins and extensive research on photocatalysis in the field of inorganic semiconductor materials carried out consecutively in the next few decades. Subsequently, numerous studies were conducted on different types of photocatalysts such as organic materials and hybrid materials. Many reviews have focused on photocatalysis and concluded that this burgeoning way of disposing plastics is appropriate from several perspectives.13,27–30 Chen et al. concentrated on the different reaction paths, advanced representative catalyst systems and converted products in their work.31 Castilla-Caballero and coworkers introduced various photocatalysts in a chronological order and further evaluated the degree of plastic degradation using techniques such as weight loss, molecular weight determination and carbonyl index.32 Chu et al. emphasized the transformation from plastics to materials, chemicals and access fuels through selective C–C and C–H bonds.22 Du et al. classified solid wastes and elaborated the strengths of cooperatively coupling hydrogen production with the photodegradation of solid wastes.30 Karimi et al. demonstrated the post-synthetic modifications of plastic wastes to improve the degradation effect and acquire the desired products.33 Zheng and coworkers divided state-of-the-art techniques into two categories, and summarized several catalysis methods with their present situations and potential applications.34 Zhang et al. reviewed solar-driven catalytic plastic upcycling under mild conditions. They also discussed how to precisely and selectively produce high value-added chemical products.35 However, little attention has been given to the classification of photocatalysis based on the constituents and the recent advancements in achieving the intended effect of photocatalytic degradation of plastics and enhancing the feasibility of its widespread application.
In this review, we focus on studies on different types of photocatalysts and various means of optimizing the photocatalysis performance. This review aims to provide an organized and systematic overview of the progress achieved in the photocatalysis of (micro)plastics, exploring aspects that may affect the processes and outcomes of photocatalysis and considering the current limitations and future perspectives in photocatalysis. It is believed that photocatalysis technologies for the degradation of (micro)plastics can achieve significant commercial and environmentally friendly potential in the future.
Polymer type | Degree of crystallinity | Tensile strength (MPa) | Elongation at break (%) | Flexural modulus (GPa) | Typical products and applications | Ref. |
---|---|---|---|---|---|---|
HDPE | High | 20–30 | 10–1000 | 1–1.5 | Milk bottles, wire and cable insulation, and toys | 41 |
LDPE | Moderate | 8–30 | 100–650 | 0.25–0.35 | Packaging files, grocery bags, and agricultural mulch | 42 |
PVC | Nil | 40–50 | 2–80 | 2.1–3.4 | Pipes, conduits, and home siding, window frames | 43 |
PP | High | 30–40 | 100 = 600 | 1.2–1.7 | Bottles, food containers, and toys | 44 |
PS | Nil | 35–50 | 1–2 | 2.6–3.4 | Eating utensils, and foam food containers | 45 |
Currently, under the promotion of plastic restriction, heterochain polymers, which are well-known as biodegradable plastics, have become a type of environmentally friendly material with high demand in the market.46 Compared with traditional plastics, they are non-toxic, harmless and can be metabolized by microorganisms in the natural environment and degraded swiftly into small molecules such as CO2, H2O and methane.47 According to the composition and preparation method of raw materials, biodegradable plastics can be divided into natural polymer degradable plastics, microbial synthetic degradable plastics, ad chemical synthetic degradable plastics.48 At present, the biodegradable plastics that are well developed and employed on an industrial scale to a certain degree mainly include polylactic acid (PLA), poly(butylene succinate) (PBS), poly(butylene succinate-co-butylene adipate) (PBSA), poly(butylene adipate-co-terephthalate) (PBAT), polyhydroxyalkanoate (PHA), polypropylene carbonate (PPA), polyglycolic acid (PGA), and polycaprolactone (PCL).48 As substitutes for the widely used typical plastic PE, Table 2 shows the evaluation of biodegradable plastics and LDPE from different perspectives.
Plastics | Melting point (°C) | Tensile strength (MPa) | Elongation at break (%) | Degradation rate | O2 barrier property | H2O barrier property | Ref. |
---|---|---|---|---|---|---|---|
LDPE | 110 | 12 | 148 | Nil | Low | High | 42 |
PLA | 180 | 60 | 6 | Moderate | Moderate | Moderate | 49 |
PBS | 120 | 40 | 400 | Fast | — | — | 50 |
PBAT | 120 | 18 | 750 | Moderate | Low | Low | 51 |
PPC | — | 13 | 650 | Moderate | High | High | 52 |
PCL | 60 | 20 | 300 | Low | — | Moderate | 53 |
PHA | 145 | 30 | 10 | High | High | High | 54 |
PGA | 225 | 80 | 10 | High | High | High | 55 |
To some extent, biodegradable plastic can indeed alleviate the white pollution problem that has plagued human beings for a long time,47 but it still has many problems at present. Firstly, the degradation conditions of biodegradable plastics are harsh given they can only be rapidly degraded under compost conditions.56 Secondly, most biodegradable plastics are made from food. Taking PLA as an example, it is made from corn starch or the sugar found in sugar cane and sugar beets.57 Thus, if the situation does not improve, there will be less food available for humans to eat in the future if the production of biodegradable plastics continues to increase, leading to a severe food race between plastics and humans. Thirdly, the prohibitive cost of biodegradable plastics will be a significant factor limiting their use for at least five years.58
Microplastics are classified depending on the path through which they enter the natural environment and ecosystem.72 Primary microplastics are products manufactured specifically as mentioned above, which enter the terrestrial ecosystem through atmospheric deposition and their employment in agricultural lands.73 Secondary microplastics come from larger plastics that break into small pieces with the help of physical, chemical, mechanical and biological activities.73 Microplastics originating from the improper disposal of plastics are mostly secondary microplastics, which occupy a large proportion in the environmental network.73 Despite the small size of microplastics, similar to plastics, they still take hundreds or even thousands of years to decompose, leading to a greater biohazard especially to freshwater ecosystems and marine organisms.74 When microplastics enter the soil system, they cause great harm directly or indirectly by interacting with or absorbing organic or inorganic toxins, and then disperse in the soil, thus affecting the polymer composition, oxygen concentration and pH value.75 These factors are essential for the survival of microorganisms and plants in soil and further enter the food chain, posing a risk to all creatures. Even worse, during the aging process, different types of chemicals including phthalates, phenols, and acetophenones can be discharged and long-lasting negative effects are consecutively triggered.75
When plastics are disposed in the presence of photocatalysts, briefly, their degradation can be attributed to the following procedures: (i) capturing energy from light to produce electron–hole pairs, (ii) aggregating charge from the interior homogeneous dispersal of the photocatalysts to the surface, and (iii) triggering the redox reactions with the actuation of charges at the interface between reactants and photocatalysts.78–80 When the photocatalyst absorbs light with sufficiently high energy, electrons are excited from the valence band to the conduction band, e(CB)−, and subsequently holes are formed on the valence band, h(VB)+.81 One strategy for photocatalytic reaction is conducted in an oxygen-rich atmosphere, which is called the O2 evolution reaction (OER).82 During the degradation process, O2 reacts with free electrons and is reduced to superoxide anion radicals, O2˙−, in the valence band. Simultaneously, the holes in the valence band migrate to the surface and react with H2O to form hydroxyl radicals, ˙OH, or directly with (micro)plastics (eqn (1)–(3)).83 Then, the superoxide radicals, O2˙−, react with the e(CB)− and H+ produced from H2O to form hydrogen peroxide (eqn (4)), which further reacts with photons, superoxide radicals, O2˙−, and e(CB)− to form hydroxyl radical ˙OH, OH− and O2 (eqn (5)–(7)), respectively. Superoxide radicals, O2˙−, and hydroxyl radicals, ˙OH, are among the most active photocatalytic oxidants, which can efficiently oxidize organic compounds (eqn (8)).84,85 OER photodegradation treats (micro)plastics as wastes to be degraded and generates highly oxidizing radical species, subsequently leading to nonselective oxidation reactions.86,87
Another type of photocatalytic reaction is carried out in inert atmosphere, usually in N2 or Ar, which is usually called the H2 evolution reaction (HER).88 In this case, (micro)plastic wastes function as misplaced hydrocarbon resources, enabling the production of value-added products and H2.22 Different from photodegradation with O2, the holes generated by photons on photocatalysts drive the transformation of (micro)plastics to produce relatively highly selective value-added chemicals (eqn (11)), while the photoinduced electrons react with protons simultaneously to form H2 (eqn (10)).89,90 The overall photocatalytic reaction process of (micro)plastics of these two different strategies is summarized in Table 3, and Fig. 2 illustrates their mechanism briefly.
Photocatalytic reactions in oxygen-rich atmosphere: | |
---|---|
Photocatalyst + hv → h(VB)+ + e(CB)− | 1 |
O2 + e(CB)− → O2˙− | 2 |
H2O + h(VB)+ →·OH + H+ | 3 |
O2˙− + 2H+ + e(CB)− → H2O2 | 4 |
H2O2 + hv → 2˙OH | 5 |
H2O2 + O2˙− → ˙OH + OH− + O2 | 6 |
H2O2 + e(CB)− → ˙OH + OH− | 7 |
˙OH or O2˙− + (micro)plastics → intermediates + products | 8 |
Photocatalytic reactions in inert atmosphere: | |
---|---|
Photocatalyst + hv → h(VB)+ + e(CB)− | 1 |
H2O + h(VB)+ → ˙OH + H+ | 9 |
H+ + e(CB)− → H2 | 10 |
h(VB)+ or ˙OH + (micro)plastics → Selective valuable organic products | 11 |
The photocatalytic effect is greatly related to the bandgap of photocatalysts, which can dominate the beginning and ending of the reaction process. A narrower bandgap allows (micro)plastic degradation to be conducted in a more facile way, and thus a broader range of materials can be chosen as photocatalysts. For example, TiO2 and ZnO have bandgaps of 3.2 eV,91,92 while that of C3N4 is 2.7 eV, CN-CNTs-NM is 2.4 eV,93 polypyrrole (PPy) is 2.2 eV, V-substituted phosphomolybdic acid (VPOM) is 2.19 eV,94 and PET-derived carbon nitride sheets (PCNS) is 1.82 eV.95 During degradation, the measured activation energies vary with different properties. In the case of HDPE, the activation energy is in the range of 85.6 ± 27.6 kJ mol−1 for the formation of a carbonyl group and 71.5 ± 8.9 kJ mol−1 for the formation of vinyl.96 Meanwhile, in the case of LDPE, the reported activation energy for carbonyl formation fluctuates in the range of 46 kJ mol−1 to 95 kJ mol−1. For other degradation products, namely vinyl and hydroxyl groups, the activation energies are lower, which are between 20 kJ mol−1 and 46 kJ mol−1.97–99 The Gibbs energy changes (ΔG0) have also been reported in some studies. For example, the ΔG0 for the reforming of lactic acid (a monomer of PLA) is +27 kJ mol−1, while that for ethylene glycol (a monomer of PET) is +9.2 kJ mol−1.100,101 In general, plastic disposal requires a lower potential, hence lowering the total potential required to accomplish the OER and HER reactions, making photocatalytic degradation more accessible.22,101 Under this condition, plastic wastes are similar to sacrificial agents, which are easily oxidized by superoxide radicals, hydroxyl radicals or low energy photoinduced holes.22
For most doped semiconductors such as Fe/Ag-doped TiO2, the dopants serve as traps of both h(VB)+ and e(CB)−, aiming to avoid the recombination of electron/hole pairs.102 Also, semiconductors with other surface modifications can increase the degradation rate because the composite extends the light absorption to the visible spectral region. In these case of hybrid catalysts such as CuPc–TiO2 and FePc–TiO2, the dye sensitization is firstly excited to generate e(CB)− and h(VB)+, and then the electron is shifted to the conduction band of TiO2 and lead to next series of oxidation–reduction reactions. Additionally, these composites can effectively prevent the aggregation of semiconductors on polymers due to their particular microstructure.103 Benefiting from these features, composite photocatalysts can achieve a uniform dispersion, higher stability and relatively higher degradation rate compared to other catalysts.
Cat. type | Photocatalyst | Plastic | Light source | Time | Degradation efficiencya [%] | Ref. | |
---|---|---|---|---|---|---|---|
Weight loss | Other | ||||||
a Different papers present the degradation rate through different indices. Below we list the results with the data provided in the references and the index is remarked respectively. b NMR yield of benzoic acid. c Total yield of benzoyl products on a monomer basis. d Selectivity (%) = (n(carbon in benzoic acid, acetophenone and benzaldehyde)/(n(carbon in benzoic acid, acetophenone and benzaldehyde) + n(COx total))) × 100%, COx from solvent oxidation is included. e Conversion (%) = 100 × Nlim/N100%, Nlim is the limiting amount of H2 obtained from 1 mol of substrate. N100% is the ideal amount of H2 obtainable from 1 mol of substrate (calculated from chemical reactions listed in the main text). f AQY (%) = (number of reacted electrons)/(number of incident photons) = (2 × number of evolved hydrogen molecules)/(number of incident photons) × 100%. g Upcycling efficiency, defined as the carbon element recovery efficiency after 36 h reaction: the moles of produced formic acid divided by the moles of carbon atoms in the added plastic. h Degradation efficiency. | |||||||
Inorganic | TiO2 | PVC | Simulated sunlight | 300 h | 27 | 104 | |
Fe/Ag mix doped TiO2 | PE | UV light | 300 h | 14.34 | 105 | ||
Ag doped TiO2 | PE | Artificial light | 300 h | 14.28 | 105 | ||
BiOI/TiO2 | PVC | UV light | 336 h | 30.8 | 106 | ||
TiO2-MWCNTs | PE | UV light | 180 h | 35 | 107 | ||
OMS-2 | PE | UV light | 288 h | 16.5 | 108 | ||
ZnO | PS | UV light | 2 h | 16 | 109 | ||
B–goethite | PE | UV light | 300 h | 12.6 | 110 | ||
FeCl3 | PS | Blue LED | 48 h | 78b | 111 | ||
FeCl3 | PS | White light | 20 h | 23c | 112 | ||
Fe2(SO4)3 | PS | LED | 66 h | 63b | 112 | ||
C3N4 | PS | 300 W Xenon lamp (150 °C) | 24 h | 60 ± 4d | 113 | ||
CdS/CdOx QDs | PLA | Simulated solar light | 24 h | 38.8 ± 4e | 114 | ||
CNx|Ni2P | PET | Simulated solar light | 8 days | 24.5 ± 3.3e | 100 | ||
CN-CNTs-NM | PET | LED (288 K) | 4 h | 0.62f | 93 | ||
VPOM/CNNS | PEG | Visible light | 3 h | 16.55g | 115 | ||
Organic | Fluorenone | PS | Blue LED | 48 h | 38 ± 3b | 116 | |
pTsOH·H2O | PS | 450 nm, 9 W | 15 h | 50b | 117 | ||
Hybrid | FePc–TiO2 | PS | Sunlight | 12 days | 35 | 103 | |
PPy/TiO2 | PE | Sunlight | 240 h | 35.4 | 118 | ||
FePcCl16-TiO2 | PVC | UV light | 240 h | 50 | 119 | ||
PAM-g-TiO2 | LDPE | UV light | 520 h | 39.85 | 120 | ||
T@AIH | LDPE | 340 nm Xenon lamp (65 °C) | 72 h | 54.7h | 78 |
In 2001, Cho et al. studied the photocatalytic degradation of PVC films embedded with TiO2 particles (0–2 wt%) under ambient air or a nitrogen atmosphere using SEM microscopy, FT-IR and UV-vis spectroscopy, and XPS (Fig. 3).104 In these experiments, the PVC–TiO2 composite films consisted of 1.5 wt% of TiO2 and were 25–30 μm thick, which were irradiated under a 200 W mercury lamp. According to the results, the weight of the PVC–TiO2 film decreased by 27% with irradiation under air, while the PVC film showed only 10% weight loss under identical experimental conditions. Cho et al. reported that the Mw of the composite film steadily decreased with irradiation time. During the process of photodegradation, most of the higher Mw fraction disappeared after 13–15 min of elution and the average Mw was reduced to a third after 300 h irradiation. The average Mw of the pure PVC films was reduced by half in 300 h accordingly, indicating that both the direct photolytic and photocatalytic reaction participated in the bond scission in the backbone of the polymer.
Fig. 3 (a) Weight loss of the pure PVC or PVC–TiO2 (1.5 wt%) composite films during irradiation under air or nitrogen atmosphere. (b) FT-IR spectra of volatile products evolved from the irradiated PVC–TiO2 (1.5 wt%) film under air. The inset shows the evolved CO2 concentration as a function of irradiation time. (c) SEM images of the pure PVC or PVC–TiO2 (1.5 wt%) composite films. (i) PVC–TiO2 film before irradiation; (ii) PVC–TiO2 film, irradiated for 25 h; (iii) PVC–TiO2 film, irradiated for 50 h; (iv) PVC–TiO2 film, irradiated for 100 h; (v) PVC–TiO2 film, irradiated for 100 h (enlarged view); (vi) backside view of the PVC–TiO2 film, irradiated for 100 h; (vii) PVC–TiO2 film, irradiated for 100 h under N2; and (viii) pure PVC film, irradiated for 100 h. Reproduced with permission from ref. 104. Copyright 2001, Elsevier. |
The SEM images of the PVC–TiO2 composite films showed much more and larger holes on their surface under the ambient air atmosphere compared to merely no holes under a nitrogen atmosphere. This result confirmed the necessity of oxygen for the solid-phase photocatalytic reaction. The SEM images also proved that the active oxygen species generated on illuminated TiO2 diffused away from the surface into the gas-phase. Most of the oxidizing power of TiO2 is attributed to the reaction of surface hydroxyl groups on TiO2 with the valence band holes, generating hydroxyl radicals. The main gaseous products, CO2 and H2O, were monitored by using an FT-IR gas cell. Also, HCl, the main product of thermal and direct photolytic degradation of PVC, did not appear, showing that photocatalytic degradation of the PVC–TiO2 film is an environmentally friendly method.
In 2007, Bandyopadhyay et al. reported the photodegradation of polystyrene (PS) using ZnO as a photocatalyst.109 ZnO had the greatest advantage of absorbing a longer fraction of the solar spectrum, and therefore may provide the highest efficiency. The weight loss of the virgin PS as a function of UV exposure time barely increased, while the weight loss upon the addition of 0.1 wt% ZnO to PS0.1 increased, showing that ZnO acted as a photocatalyst for the degradation of PS. The weight loss of PS as a function of UV exposure time gradually increased with an increase in ZnO concentration up to 0.5 wt% with respect to PS. The 0.5 wt% ZnO-containing PS0.5 showed the highest weight loss. However, when the concentration of ZnO reached 1 wt%, PS hardly showed any weight loss under the experimental conditions. In fact, the rate of photodegradation of PS slowed down significantly when the concentration of ZnO was greater than 0.5 wt%. During the degradation, ZnO, acting as a UV absorber, could transmit the absorbed energy to the C–C and C–H bonds of the PS molecules, which caused cleavage reactions given that this energy was higher than the dissociation energies of these bonds. The dispersion of ZnO in the PS matrix was the most important factor. The better dispersion of ZnO would cause the greater absorption of the polymer macrochains on the metal oxide and higher chances of cleavage reactions by efficient energy transfer to the matrix. AFM was used to investigate the sample surface. The RMS roughness of PS0.5 after degradation reached 101 nm, which is about 7-times rougher than PS0.5 before degradation, which led by the loss of oxidized materials (mainly as CO2) from the surface upon UV exposure. The main products of the photodegradation of PS were CO2 and H2O, as reflected by the viscosity average molecular weight measurements of the degraded samples.
Liu et al. used manganese oxide (OMS-2) as a photocatalyst in the photocatalytic degradation of polyethylene (PE) in 2011.108 They studied the photocatalytic degradation of PE with OMS-2 in the ambient air under UV and visible light irradiation. During the photodegradation, OMS-2 played a vital role because of its octahedral molecular structure sieves and excellent catalytic properties. OMS-2 powder exhibited remarkable absorbance in the visible region beyond 400 nm. The weight of PE-OMS-2 (0.1 wt%) decreased by 16.5% after 288 h under UV light irradiation, while there was only 4.1% weight loss in the pure PE under the same experimental conditions. In contrast, no weight loss was observed for PE-OMS-2 under visible light irradiation after 128 h, which suggested that visible light irradiation could not induce activity for the photocatalytic degradation of OMS-2. The degradation rate is proportional to the concentration of OMS-2 when it was less than 1.0%. However, a reduction in weight loss was observed with the further addition of OMS-2. The SEM images showed the growth of cavities in the surface of PE-OMS-2 during photodegradation. An increase in the size and depth of the cavities was observed in the PE-OMS-2 films due to the escape of volatile products from the PE matrix, while few changes appeared in the pure PE film. The degradation of PE may start at the PE-OMS-2 interface, where active oxygen species generated on the surface of OMS-2 diffused and etched the polymer matrix, which led the formation of cavities around the OMS-2 particles. The OMS-2 particles irradiated by UV light generated electron/hole pairs in the conduction band and valence band, contributing to the degradation reaction.
Besides conventional semiconductors such as TiO2, ZnO and MnO, Jiao et al. achieved a 100% photodegradation rate of PE, PP and PVC into CO2 with single-unit-cell thick Ni2O5 layers, at room temperature and ambient pressure within 40, 60 and 90 h in 2020 (Fig. 4).122 Then, CO2 was further photoreduced to CH3COOH, helping to relieve the environmental pollution caused by (micro)plastics and generate value-added multi-carbon fuels simultaneously. Ni2O5 is a type of highly stable and earth-abundant semiconductor, and the fabricated single-unit-cell thick Ni2O5 can largely maximize the conducting surface, and consequently optimize the photodegradation conversion. Also, commercial PE-, PP- and PVC-based plastic commodities such as food wrap films, single-use bags and disposable food containers could also be photodegraded into CH3COOH with a smaller yield compared with pure PE, PP and PVC, indicating its possible real-world application.
Fig. 4 (a) Schematic illustration of the conversion of various waste plastics into C2 fuels by a designed two-step pathway under simulated natural environment conditions. Specifically, various plastics were exclusively degraded into CO2 by photooxidative C–C bond cleavage over a photocatalyst, while the produced CO2 was further reduced into highly valuable C2 fuels by photoinduced C–C bond coupling over the same photocatalyst. (b) Photoconversion of various plastics into C2 fuels under simulated natural environment conditions. (i) Yield of CO2 during the photoconversion of pure PE, PP, and PVC over the Nb2O5 atomic layers, in which the molar ratio of carbon in each plastic and Nb2O5 atomic layers is ca. 50:1. (ii) Yield of CH3COOH and (iii) evolution rates of CH3COOH and CO during the photoconversion of pure PE, PP, and PVC, as well as during the photoreduction of pure CO2 in water. In all the photoconversion tests, each plastic and pure CO2 have the same number of moles of carbon. (c) Schematic representation of (i) band-edge positions of Nb2O5 atomic layers along with the potentials of CO2, H2O, H2O2, and O2 redox couples at pH 7 and (ii) proposed two-step C–C bond cleavage and coupling mechanism from pure PE into CH3COOH under simulated natural environment conditions. Reproduced with permission from ref. 122. Copyright 2020, John Wiley and Sons. |
In 2022, the degradation of PS with FeCl3 was reported by Oh et al., which could promote the upcycling of PS to benzoyl products and primarily benzoic (Fig. 5).123 Under visible light irradiation, FeCl3 can generate chlorine radicals and abstract C–H bonds from the PS backbone, finally resulting in the cleavage of the C–C bond. In experiments, commercial PS was degraded. After photooxidative degradation, PS with Mw more than 90 kg mol−1 was degraded into oligomers (Mn = 0.8 kg mol−1), with up to 23 mol% generation of small-molecule benzoyl products under saturation system of O2, that is, benzoic acid, benzaldehyde, benzoyl chloride and acetophenone. Compared with benzophenone, which was used in previous research on the degradation of PS degradation, the introduction of chlorine radical in this study enhanced the formation of benzoyl products. Also, FeCl3·6H2O, LiCl, NaCl and NH4Cl were used as alternatives under identical conditions; however, no improvement in benzoyl product formation was observed.
Fig. 5 (a) Proposed upcycling of polystyrene. (b) (i) Scatter plot for benzoic acid, benzaldehyde, and benzoyl chloride at each time point for PS degradation under O2. (ii) Degradation profile of oxidized PS in the absence of FeCl3. (c) Commercial PS degradation. Reproduced with permission from ref. 123. Copyright 2022, the American Chemical Society. |
Later, in the same year, another method was proposed using heterogeneous graphitic carbon nitride (g-C3N4) as catalysts under visible light irradiation to degrade PS to aromatic oxygenates such as benzoic acid, acetophenone and benzaldehyde (Fig. 6).113 Chain oxidation happened primarily, and then the oxidized PS was cleaved. In the experiments, the exceedingly efficient upcycling of PS with the yield of 60% towards organic products was achieved. High selectivity of 74% for benzoic acid or 51% for benzaldehyde in independent experiments was achieved by adjusting the weight hourly space velocity (WHSV) of PS in a flow reaction system. In the circulatory system, with pretreated PS, at 150 °C with a proper ratio of substrate/catalyst (5:2) and reaction time (8 h), about 10 mg gcatal−1 h−1 mass-specific reactivity and over 80% selectivity towards benzoic acid were observed, indicating excellent reaction performance under the g-C3N4 photocatalyst.
Fig. 6 (a) Catalytic performances of (i) oxygen-treated polystyrene, (ii) oxygenate monomers, and (iii) hydrocarbon monomers as reactants under standard reaction conditions. Reaction conditions: 50 mg g-C3N4, 20 mg reactant, 30 mL acetonitrile, 10 bar O2, irradiated by 300 W Xenon lamp at 150 °C. (b) Proposed reaction pathway of polystyrene photo–oxidation reaction. Reproduced with permission from ref. 113. Copyright 2022, Springer Nature. |
Yang et al. improved the photocatalytic performance of nano-TiO2 by embedding a nano-TiO2 photocatalyst modified by bismuth oxyiodide (BiOI), preparing a new type of photodegradable PVC–BiOI/TiO2 nanocomposite film.106 Nano-TiO2 is considered a good photocatalyst because of its high reactivity, good photostability, low cost and non-toxicity, but it can only absorb UV light with a wavelength of less than 387 nm.124,125 Due to the heterostructure of BiOI/TiO2, the combination of nano-TiO2 and BiOI achieved more efficient separation of the electron–hole pairs and higher photocatalytic activity. The absorbance of the PVC–BiOI/TiO2 nanocomposite film was higher than that of the PVC–TiO2 nanocomposite film and pure PVC film. After 336 h UV light irradiation, the weight of the pure PVC film decreased by 3.2%. The weight loss of the PVC–TiO2 nanocomposite film reached 20.8% after 336 h of irradiation, while that of the PVC–BiOI/TiO2 nanocomposite film was 30.8%, which was 1.5-times higher than that of the PVC–TiO2 nanocomposite film. This proved that the photocatalytic performance of the nano-TiO2-containing PVC film was remarkably promoted by the BiOI modifier. They reported that the concentration of BiOI influenced the weight loss rates of the PVC–BiOI/TiO2 nanocomposite film, and when the mass ratio of BiOI to TiO2 reached 0.75%, the degradation rate reached its peak, indicating that at this time, the PVC–BiOI/TiO2 nanocomposite film had the best photocatalytic activity. When the mass ratio exceeded 0.75%, the weight loss rate decreased drastically but was still higher than that of the PVC–TiO2 nanocomposite film. The decreasing intensities of the C–H groups and the increasing intensities of the carbonyl groups shown in the FT-IR spectra of the PVC–BiOI/TiO2 nanocomposite film were more pronounced than that of the PVC–TiO2 nanocomposite film, suggesting that the photooxidation reaction occurred in the composite film. The weight loss rate of the PVC–BiOI/TiO2 nanocomposite film (TiO2: 2 wt%) changed at different mass ratios of BiOI to TiO2 under UV light irradiation.
In 2018, Uekert et al. reported the preparation of an economical photocatalyst, i.e., CdS/CdOx quantum dots, and employed it for the visible light-driven photodegradation of PLA, PET and PUR.114 After degradation, these waste plastics were converted into H2 and organic products such as formate, acetate, and pyruvate at ambient temperature and pressure. Under an N2 atmosphere, PLA, PET and PUR exhibited higher activities and could generate larger quantities of H2 compared to other types of polymers. After photocatalytic reactions, the activity for the degradation of PLA, PET and PUR was 64.3 ± 14.7, 3.42 ± 0.87, and 0.85 ± 0.28 mmolH2 gCdS−1 h−1, respectively. Individually, the overall H2 production of the three plastics reached 3.09 ± 0.15, 0.21 ± 0.04, and 0.04 ± 0.01 mmolH2 gsubstrate−1, respectively. In controlled trials without UV irradiation (λ > 400 nm), photoreforming still continued effectively, suggesting that the photocatalyst could function with the utilization of visible light ultimately.
However, this cadmium-containing catalyst makes the subsequent treatment of the plastic degradation system difficult owing to its toxicity. Then, one year later, Uekert et al. proposed the use of a nontoxic and reasonably priced carbon nitride/nickel phosphide (CNx|Ni2P) as a photocatalyst to reform PET and PLA under visible light, generating pure H2 and various organic chemicals (Fig. 7).100 Different from CdS/CdOx, this type of noble-metal- and Cd-free photocatalyst exhibited enhanced stability, catalytic efficiency and charge separation, achieving photostability for at least 5 days. Also, 82.5 ± 7.3 and 178 ± 12 μmolH2 gsub−1 H2 were produced from PET and PLA after 50 h of irradiation, with the external quantum yields of 0.035% ± 0.005% and 0.101% ± 0.018% for PLA at λ = 430 nm, respectively. The H2 conversion reached 4.4% ± 0.6% and 1.6% ± 0.2% after 8 days of photoreforming with PET and PLA, respectively. It was noted that the reaction system was still active after 8 days, indicating that the H2 conversion may achieve a higher value if the photodegradation process lasted for a longer time. Actually, the photoreforming of ethylene glycol showed 50% H2 conversions after 18 days. At a higher pH condition, elevated H2 conversions were observed as 24.5% ± 3.3% for PET and 6.7% ± 0.8% for PLA.
Fig. 7 (a) Schematic diagram of the polymer photoreforming process using CNx|Ni2P photocatalyst. (b) Characterization of the CNx|Ni2P (2 wt%) photocatalyst. Comparison of (i) diffuse-reflectance UV-vis, (ii) emission (λex = 360 nm, λem = 450 nm), and (iii) FTIR spectra of CNx and CNx|Ni2P. (iv) TEM image of the CNx|Ni2P catalyst, with the inset showing the lattice spacing of Ni2P. XPS spectra of (v) C1s edge for CNx and CNx|Ni2P and (vi) Ni2p edge for Ni2P and CNx|Ni2P. (c) Photoreforming of PET and PLA with CNx|Ni2P. Optimization of (i) Ni2P loading and (ii) KOH concentration for the photoreforming of PET (after 20 h irradiation). Black circles in (ii) mark H2 evolution per gram of substrate over CNx|Pt (2 wt%) under the same conditions. (iii) Long-term photoreforming of PET and PLA. Conditions unless stated otherwise: CNx|Ni2P 2 wt% (1.6 mg mL−1), pretreated PET (25 mg mL−1), aqueous KOH (1 M, 2 mL), and simulated solar light (AM 1.5 G, 100 mW cm−2, 25 °C). (d) Photoreforming of nonrecyclable plastic waste. (i) Long-term photoreforming of polyester microfibers, a PET bottle, and an oil-coated PET bottle. (ii) Upscaled photoreforming of polyester microfibers, where sample was purged every 24 h. Conditions: CNx|Ni2P (1.6 mg mL−1), 1 M KOH (2 mL for part (i) and 120 mL for part (ii)), pretreated microfibers (5 mg mL−1) or PET bottle (25 mg mL−1) without or with soybean oil (5 mg mL−1), simulated solar light (AM 1.5 G, 100 mW cm−2). (iii) Photograph of the batch reactor in use. Reproduced with permission from ref. 100. Copyright 2019, the American Chemical Society. |
In 2022, Gong et al. developed an in situ-derived carbon nitride–carbon nanotube–NiMo hybrid via NiMo-assisted catalysis route (CN–CNTs–NiMo), which proved to be an efficient and stable photocatalyst (Fig. 8).93 The NiMo nanoparticles acted as a co-catalyst to improve the photocatalytic activity of PET because of its excellent HER electrocatalytic activity and durability in alkaline condition. CNTs exhibited superior chemical stability, large surface area and excellent electron mobility in alkaline condition.126,127 The integration of NiMo nanoparticles and CNTs into a heterogenous structure is an effective strategy to promote the transfer of electrons from CN to NiMo. According to their study, the strong π–π interactions between CNTs and CN can promote electron transfer from CN to NiMo, increase the carrier lifetime and improve the photocatalytic activity. The photocatalytic activity of CN–CNTs–NiMo for the photodegradation of PET was around 14 times higher than that of CN. After normalization to exclude the influence of the surface area of the photocatalyst, CN–CNTs–NiMo still showed nearly 2-times higher hydrogen evolution rate with PET than CN.
Fig. 8 (a) (i) XRD patterns of CN, CN–NM, CN–CNTs–NM and CNTs–NM. (ii) SEM images of CN–CNTs–NM. (iii) Low-magnification TEM and (iv) HRTEM image and SAED pattern of CN–CNTs–NM. (v) N2 adsorption desorption isotherms of CN–CNTs–NM and CN. (b) Schematic diagram of the process of photoreforming of PET using CN–CNTs–NM. (c) (i) 1H NMR spectra of PET before and after photoreforming. (ii) Photoreforming of PET to obtain commodity chemicals and H2 fuel. Reaction conditions: 10 mL KOH (5 M), pretreated PET (50 mg mL−1), and 10 mg CN–CNTs–NM under simulated solar light for 4 h at 288 K. Light resource: simulated solar light, 95 mW cm−2. Reproduced with permission from ref. 93. Copyright 2022, Elsevier. |
Also, based on the advantages of carbon nitride, C3N4, Xing et al. designed and fabricated a self-assembly Z-scheme heterostructure of V-substituted phosphomolybdic acid clusters/g-C3N4 nanosheets (VPOM/CNNS), which is an efficient and sustainable strategy for the photodegradation of various plastic waste under visible light irradiation (Fig. 9).115 The bio-mimic Z-scheme heterostructure not only promoted the carrier separation, but also reserved the strong redox ability of electrons and holes to participate in the photodegradation of plastics. The VPOM/CNNS Z-scheme heterojunction exhibited abundant surface-active sites and short charge transport by rationally modulating the surface charge. VPOM/CNNS could photodegrade various polymers to produce formic acid (HCOOH), which has a wide range of applications in fuel cells and liquid storage for hydrogen energy. The best formic acid production rate of the VPOM/CNNS composite was up to 24.66 μmol h−1 g−1, which was 262-times higher than that of pristine CNNS.
Fig. 9 (a) (i) Schematic diagram of VPOM/CNNS heterojunction prepared via electrostatic self-assembly process. (ii) TEM images and (iii) AC-HAADF-STEM image of VPOM/CNNS-15 hybrid. (iv) Optimized model of VPOM cluster by theoretical calculation. (v) AC-HAADF-STEM image of VPOM/CNNS-15 hybrid. (vi), (vii), and (viii) Intensity profile of the selected circled area in (v). (b) DFT calculations for the molecular orbits of (i) VPOM cluster and (ii) CNNS model (the left, middle and right columns represent the ball-and-stick representation, HOMO and LUMO orbits, respectively). (iii) Schematic of the photocatalytic upcycling process for VPOM/CNNS Z-scheme heterojunction. (iv) Proposed reaction mechanism for photocatalytic upcycling of plastics by the oxidative C–C bond cleavage with VPOM/CNNS hybrid. (c) (i) Photocatalytic upcycling of polyethylene and (ii) bar chart of HCOOH production rates for 36 h irradiation of samples. (iii) Long-term photocatalytic test of VPOM/CNNS-15 for photocatalytic upcycling of polyethylene. (iv) Photocatalytic upcycling of real-world plastic waste over VPOM/CNNS-15. (v) Photocatalytic upcycling of polyethylene with different scavengers of VPOM/CNNS-15. (vi) ESR spectra of reaction mixtures in different reaction conditions. Reproduced with permission from ref. 115. Copyright 2022, Elsevier. |
In 2022, Huang et al. first described a light-driven, acid-catalyzed protocol for the degradation of polystyrene under mild conditions without the need for photosensitizers (Fig. 10).133 They found that triflic acid (5 mol%, HOTf) could catalyze the photodegradation of PS under 405 nm violet-blue light irradiation with 1 bar O2 as the oxidant. The products of the photodegradation of PS were isolable formic acid with 72% yield, benzoic acid with 40% yield and benzophenone with 2% yield. Since there were no desirable products without irradiation, light played a significant role in the degradation. This group also found that methanesulfonic (CH3SO3H) and p-toluenesulfonic acid monohydrate (pTsOH·H2O) can afford the corresponding products.
Fig. 10 (a) Computational study of the hydrogen atom transfer (HAT) reaction of 1,3-diphenylbutane 7 with various oxygen speciesa (aall energies were calculated at the B3LYP-D3/6-311+G (d,p)/SMD (acetonitrile)//B3LYP-D3/6-31G(d) level of theory). (b) Degradation of PS enabled by photocatalysis in flow: (i) optimized setup and conditions and (ii) gram–scale reaction (note: E-series system from Vapourtec was used for this transformation). (c) UV-vis spectra of PS, pTsOH·H2O, mixture of PS and acid (pTsOH·H2O, H2SO4, or HOTf), and the byproduct ([PS]: 10 mM (based on single repeat unit); [acid]: 10 mM; [byproduct]: 1 mg mL−1, in DCE). Reproduced with permission from ref. 133. Copyright 2022, the American Chemical Society. |
A photocatalyst with high activity, polypyrrole/TiO2 (PPy/TiO2), was prepared via sol–gel and emulsion polymerization by Li et al. in 2010.118 After 240 h sunlight irradiation, the weight loss rate of PE-PPy/TiO2 was 35.4%, which was much higher than that of 11.7% for PPy and 3.2% for TiO2. By coating the PPy conducting polymer, the crystalline structure of TiO2 was maintained and the visible light capturing ability of TiO2 was enhanced, accounting for the highly enhanced photocatalytic activity of PPy/TiO2.135 In 2011, Fa et al. applied TiO2 nanoparticle-modified perchlorinated iron(II) phthalocyanine (FePcCl16) as a photocatalyst for the photodegradation of a poly(vinyl chloride) (PVC) composite.119 The FePcCl16–TiO2 composite exhibited a remarkable absorbance in the visible region beyond 400 nm, while blank TiO2 could only absorb UV light and hardly absorbed light beyond 400 nm. The weight loss rate of the PVC–FePcCl16–TiO2 film reached 50% after 240 h irradiation under UV light, which was much higher than 30% weight loss rate of the PVC–TiO2 film under the same condition. Under 15 days of solar light irradiation experiment, the weight loss rate of the PVC–FePcCl16–TiO2 film was 81%, which was 80% higher than that of the PVC–TiO2 film. The PVC–FePcCl16–TiO2 film showed a higher photodegradation efficiency under both sunlight irradiation and UV light irradiation.
Liang et al. prepared a photocatalytic polyacrylamide-grafted TiO2 (PAM-g-TiO2) nanocomposite and studied the photodegradation of LDPE/PAM-g-TiO2.120 The weight loss rate of LDPE/TiO2 was 30.63% under 520 h UV light irradiation. The weight of the LDPE/PAM-TiO2 composite film decreased by 39.85% under 520 h UV light irradiation and its average molecular weight was reduced by 94.60%. By introducing PAM on TiO2 particles, good dispersion and hydrophilicity are expected to appear in the LDPE matrix. The reaction between TiO2 and the adsorbed H2O in the PAM phase led to an increase in hydroxyl radicals, which initiated the degradation of LDPE.
In 2021, Zhao et al. designed a new photocatalyst, TiO2@amylose/polyiodide/hydroxyethyl cellulose (T@AIH), for the first time, achieving not only a tunable and stable stage, but encouraging self-colour-changing property and a self-indicating delayed onset of operation (Fig. 11).78 The particular self-colour-changing property fits well with the beginning of the active stage of degradation, from blue to white, which profits from the addition of hydroxyethyl cellulose (HEC). After 72 h irradiation with the T@A0.1IN photocatalyst, LDPE-CP was oxidized, where the carbonyl index (CI) was 0.6556, and mineralized into CO2. The weight average molecular weight (Mw) of LEPE-CP experienced a reduction from 233105 g mol−1 to 206370 g mol−1. Similarly, the number average molecular weight (Mn) decreased from 26234 g mol−1 to 1462 g mol−1. The decrease in Mw and Mn indicates the chain breakage reaction of LDPE, suggesting the degradation of the polymer.
Fig. 11 (a) Photodegradation reaction with newly designed photocatalyst T@AIH. (b) Photocatalytic performance of T@H, T@AI, TiO2, and T@AIH on phenol degradation and adsorption performance of T@AIH on phenol. (c) SEM images of TiO2 (i), T@AIH (ii), UV-vis absorption spectrum of T@AIH (iii), and TGA curve of T@AIH (iv). Bottom left inset in (iii) is the digital graph of T@AIH. Reproduced with permission from ref. 78. Copyright 2021, Elsevier. |
Besides TiO2, C3N4 is also commonly employed in the research on hybrid photocatalysts. Sun et al. proposed the use of a benzenesulfonyl chloride-incorporated g-C3N4 (BS–CN), which is a novel intramolecular donor–acceptor conjugated g-C3N4 (Fig. 12).136 This synthesis extended the π-electron delocalization, narrowing the bandgap and strengthening the absorption in the visible light region, and consequently enhanced the photocatalytic performance significantly. The indirect band gap of CN and BS5–CN are 2.75 and 2.54 eV, respectively. The grafting of the electron acceptor BS on the CN framework also accelerated the electron transmission and increased the efficiency of the separation of photoexcited electron–hole pairs. Using PLA dispersed in KOH solution as a sacrificial reagent in this work, the H2 production rate employing Pt-loaded (1 wt%) BS5–CN was optimized to roughly 1.8-times higher than pure g-C3N4, which was 1890 μmol h−1 g−1 under visible light irradiation, at 40 °C for 24 h. Simultaneously, lactate was oxidized into formate and acetate, achieving the transformation of PLA plastic wastes into high-added-value chemical products and clean hydrogen energy, relieving the environmental pollution and energy dilemma.
Fig. 12 (a) UV-vis DRS and Tauc plots (i), Mott–Schottky plots (ii), and band position (iii) of CN and BS5–CN. (b) Effect of the concentration of KOH solution for hydrolysis of PLA with course (inset) and rate of H2 generation in the presence of BS5–CN(i), time course (inset) and rate of H2 production over CN and BSx-CNs using the hydrolysate of PLA, hydrolyzed in 1 M KOH solution, as the sacrificial reagent, and SBET of CN and BSx–CNs (ii), photocatalytic stability of BS5–CN(iii), and AQE of BS5–CN under three different wavelengths of monochromatic light (λ = 420, 450, and 500 nm) (iv). (c) Mechanism of photocatalytic production of H2 and organic chemicals over BS–CN from lactate solution. Reproduced with permission from ref. 136. Copyright 2021, Elsevier. |
In 2022, Han and coworkers focused on carbonized polymer dot-graphitic (CPDs-CN) catalytic solar-driven PET upcycling, together with H2 production.137 In this work, PET was used as a valuable feedstock to produce high-value-added products, which were mainly glycolic acid, glycolaldehyde and ethanol, together with H2 produced from water splitting. The yield of terephthalic acid reached 304.7 ± 17.2 μmol and the production rate of H2 achieved was 1034 ± 134 μmol g−1 h−1, which showed promising application towards the sustainable production of added-value solar chemicals and fuels.
Thus, to address this limitation, better photocatalytic efficiency can be obtained by systematically exploring photocatalysts. One of the efficient ways is the combination with other metal/non-metal dopants to enhance the photocatalyst capacity. For example, Asghar et al. prepared four types of composite films of PE undoped, Fe-doped, Ag-doped and Fe/Ag mix-doped TiO2 nanoparticles to research the photocatalytic degradation.105 The results demonstrated that compared to the PE-TiO2 films without dopants, the other three composite films showed a more positive effect on weight reduction under the same experimental conditions (Fig. 13a).
Fig. 13 (a) Effect of UV irradiation on the photocatalytic degradation of PE films. (b) SEM images of PE films before and after irradiation: (i) PE film before irradiation, (ii) PE film after irradiation, (iii) PE-TiO2 film after irradiation, (iv) PE-Fe doped TiO2 film after irradiation, (v) PE-Ag-doped TiO2 film after irradiation, and (vi) PE-Fe/Ag mix-doped TiO2 film after irradiation. Reproduced with permission from ref. 105. Copyright 2011, Hindawi Publishing Corporation. (c) Weight loss of PE, P25-PE and TiO2-MWCNT-PE films with different MWCNT contents under UV irradiation in air. (d) Optical microscopy images of the TiO2-MWCNT (20 wt%)-PE film before (i) and after (ii) irradiation. The objective magnification is 40×. Reproduced with permission from ref. 107. Copyright 2014, Elsevier. |
Besides, as a result of photodegradation, cavities appeared randomly on the surface of the composite films, which were caused by the escape of volatile products from the PE matrix. It was be observed that the PE-TiO2 film had massive cavities,142 while the composite films doped with metal had larger cavities, showing a rough shape (Fig. 13b). This strongly demonstrated that the photocatalytic plastic degradation capability of TiO2 doped with metals is more efficient than that of undoped TiO2. In addition, the effect of the mixed doping of the PE-TiO2 composite film was midway between the Fe-doped and Ag-doped PE-TiO2 films. This indicated that photocatalysts with some specific requirements can be obtained by adjusting the ratio of doped metal ratios. Similar results were found in the studies by Thomas et al.,143 Zhao et al.,144 and Gonçalves et al.145
An et al. investigated the photocatalytic degradation of TiO2-MWCNTs-PE films with MWCNT weight contents of 5 wt%, 10 wt%, 20 wt% and 40 wt% by weight loss analysis under mercury lamp irradiation in the ambient air.107 After 180 h irradiation under identical experiment conditions, the weight reduction of four films with different mass ratios of MWCNTs was 28%, 29%, 35% and 24% respectively, among which the TiO2-MWCNT (20 wt%)-PE composite film showed the highest photodegradable efficiency (Fig. 13c). Also, the optical microscopic images of the TiO2-MWCNT (20 wt%)-PE composite film before and after irradiation indicated that assorted sizes of cavities and holes appeared around the photocatalyst particles (Fig. 13d).
As the exposure time prolonged, it was evident that the photodegradation efficiency of the composite films increased with an increase in the MWCNT mass ratio ranging from 5 wt% to 20 wt%, while that for the TiO2-MWCNT (40 wt%)-PE composite film was the opposite. Their research confirmed that by adjusting the loading of MWCNTs, the optimal photodegradation efficiency could be achieved. Many other studies showed the advantages of MWCNTs, which proposed that they can be used as photosensitizers to broaden the absorption band of TiO2 to the visible spectrum, thereby improving the efficiency of photocatalysts.146,147 Moreover, the particle size and morphology of photocatalysts also affect the photocatalytic rate. For instance, Kamrannejad et al. studied the factors affecting the photocatalytic degradation behavior of carbon-coated TiO2 nanotubes in polypropylene (PP)-based nanocomposites, including particle size and thickness of the carbon layer.148 A thicker carbon layer reduced the penetration of UV light,149,150 which decreased the photocatalytic efficiency. Also, with an increase in particle size, the interfacial area between PP and the TiO2 reduced, leading to the lower photocatalytic efficiency.151
Besides conventional inorganic semiconductor-based composites photocatalysts, researchers also turned their attention to organic and hybrid photocatalysts.116,119,120 In the case of organic photocatalysts, the selective addition of acids (sulfuric acid (H2SO4), nitric acid (HNO3), perchloric acid (HCIO4), etc.) to the reaction process is usually employed to improve the efficiency for the photodegradation of plastics and the yield of recyclable products. These additional acids played a significant role in the oxygen reduction reaction and removing excess H2O generated during the reaction. Besides, to achieve selective oxidation or cleavage of C–H bonds, hydrogen atom transfer (HAT) catalysts are often added.152,153 For hybrid photocatalysts, the most important thing is to regulate the concentration of suitable hybridizer, which may reduce the efficiency of photodegradation plastic reaction if it is too high or too low.
Fig. 14 (a) (i) Conversion of 500 mg plastic pellets in 20 reaction cycles, reaction conditions: 200 mg g-C3N4, 500 mg pellets, 40 mL acetonitrile, 10 bar O2, irradiated by 300 W Xenon lamp at 150 °C for 8 h in each cycle. The solution is released after each cycle and pure solvent is injected in the autoclave. (b) Catalytic performance of polystyrene with different pretreatment, reaction conditions: 50 mg g-C3N4, 20 mg polystyrene, 30 mL acetonitrile, irradiated by 300 W Xenon lamp at 150 °C for 8 h. PS-O was obtained by thermal treatment at 150 °C in acetonitrile with O2, PS-1 and PS-2 were obtained by air treatment at 220 °C and 300 °C, respectively, and PS-3 was obtained by pyrolysis at 350 °C in N2. Reproduced with permission from ref. 113. Copyright 2022, Springer Nature. (b) Plausible mechanism of the reaction. Reproduced with permission from ref. 111. Copyright 2021, Wiley-VCH. (c) (i) UV-vis absorption spectra of PCNS and CN; the insets show photographs of PCNS and CN. (ii) Plots of transformed Kubelka–Munk function versus the energy (hv) of absorbed light for PCNS and CN. (iii) XPS VB spectra and (iv) band structures of PCNS and CN. Reproduced with permission from ref. 95. Copyright 2022, Elsevier. |
The pretreatment of plastics seems to be a small step, but it contributes greatly to the improvement of the efficiency and product selectivity of the photocatalytic reaction system.
Alternatively, Liu et al. engineered a novel carbon nitride (C3N4)-based donor–acceptor (D–A) conjugated copolymer.95 The aromatic ring was incorporated in the C3N4 skeleton to form the structure through the copolymerization of melamine and terephthalic acid obtained from the degradation of waste PET catalyzed by ZnO at 360 °C. They prepared PET-derived C3N4 sheets (PCNS) and used C3N4 (CN) for comparison. Compared with pristine CN, the synthesis of the intramolecular D–A conjugated structure strongly promoted the migration and separation of charge carriers, significantly enhanced the ability of capturing visible light (Fig. 14c) and made the C3N4-based D–A conjugated copolymer photocatalysts exhibit better photoinduced charge transfer efficiency. Besides, the special structure greatly narrowed the band gap and enhanced the carrier mobility. These results have been confirmed by many other studies.161–164 Through the transformation, structure modification and copolymerization of the products during the photodegradation of waste plastics, more efficient photocatalysts can be obtained, which is conductive to the sustainable development and recycling of resources.
The adjustment of reaction conditions involves the use or modification of intermediates and products to achieve the more efficient photocatalytic degradation of plastics or recycling plastic waste for industrial manufacturing, which is killing two birds with one stone.
Fairbrother et al. investigated the effects of environmental factors on the performance of photodegradable high-density polyethylene (HDPE) under a range of laboratory conditions, including three temperature levels (30 °C, 40 °C, and 50 °C), six UV irradiation levels from a metal halide light source (153 W m−2, 61 W m−2, 38 W m−2, 15 W m−2, 8 W m−2 and 0 W m−2) and two humidity conditions (<5% relative humidity (RH) and 75% RH).96 According to the results, an increase in temperature and UV intensity tended to accelerate the change of the mechanical properties of HDPE. The retained elongation-at-break of HDPE under harsher conditions with the same exposure time was larger, and the change rate of mechanical properties was faster (Fig. 15a), and thus the surface crystallinity index for HEDP (Fig. 15b). The overall conclusions were consistent with that in other reports.167–170 Nevertheless, there was no significant difference between the two humidity conditions for HDPE, possibly because of its high hydrophobicity.
Fig. 15 (a) Retained elongation-at-break as a function of exposure time (i) at 30 °C, 40 °C, and 50 °C with 40% UV irradiance and (ii) at 50 °C with 0%, 5%, 10%, 25%, 40%, and 100% UV irradiance. (b) Surface crystallinity index for HDPE as a function of exposure time (i) at 30 °C, 40 °C, and 50 °C with 40% UV irradiance and (ii) at 50 °C with 0%, 5%, 10%, 25%, 40%, and 100% UV irradiance. Reproduced with permission from ref. 96. Copyright 2019, Elsevier. (c) Weight loss of the composite films under UV light irradiation in (i) dry air and (ii) humidified air. Reproduced with permission from ref. 103. Copyright 2008, Elsevier. |
Similarly, they left HDPE exposed outdoors in southern Florida in the United States and examined it periodically during exposure to quantify the effect of each environmental factors on the photodegradation on HDPE through the change in performance. In this case, outdoor conditions are more diverse and complicated, making it difficult to compare with the laboratory environment. Under outdoor exposure conditions, the brittle failure time was over two times longer than that under accelerated laboratory conditions. The rate of performance change outdoors did not easily match that seen in the laboratory due to the spectral differences and cyclic changes in the outdoor environment. Up to the end of the exposure period, the variation in mechanical properties well matched the variation in laboratory exposure at 40 °C and 50 °C.
The values of retained elongation-at-break, yield stress, modulus of elasticity and crystallinity indices outdoors were close to that at 40% UV exposure in the laboratory experiment at the two higher temperatures studied. The fact that the mechanical properties measured at embrittlement matched the values under laboratory conditions positively implied that the photodegradation pathway is similar in the laboratory and outdoor environment.
Furthermore, Fa et al. revealed the effect of water vapor of a novel photodegradable PS–FePc–TiO2 nanocomposite film under humidified air and dry air.103 The weight loss of the composite film was greater in a higher humidity environment, whereas it was only one-third of that in dry air (Fig. 15c). This proposed the physical adsorption of a certain amount of water is essential for the photodegradation of PS films. These conclusions were also similar to that in other reports.171–173
In most scenarios, plastic is treated as household waste and pollution. Consequently, to realize the wide practical application of the photocatalytic degradation of plastics, the influence of environmental factors should be considered.
Briefly, the optimization of the photocatalytic degradation of plastics requires the overall improvement of photocatalysts, reactors and reaction media. To realize the overall disposal of plastics and microplastics through photocatalysis, more research should be conducted to achieve commercial success, together with the technique being suitable for mass manufacture. Moreover, great physical and mechanical properties corresponding to typical plastics should also be achieved based on environmental protection. Accordingly, photocatalysis can become widespread and gradually replace conventional plastics or conservative strategies of disposing plastics. Photocatalysis is quite promising in degrading plastics and we believe that it can be widely applied one day.
Footnote |
† These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2023 |