Kai Yu
Wang
a,
Martin
Weber
b and
Tai-Shung
Chung
*ac
aDepartment of Chemical & Biomolecular Engineering, National University of Singapore, 4 Engineering Drive 4, 117585, Singapore. E-mail: chencts@nus.edu.sg; Fax: +65-67791936; Tel: +65-65166645
bAdvanced Materials & Systems Research, BASF SE, RAP/ES-B001, 67056 Ludwigshafen, Germany
cGraduate Institute of Applied Science and Technology, National Taiwan University of Science and Technology, Taipei 106335, Taiwan
First published on 14th March 2022
As an attractive candidate material, polybenzimidazole (PBI) has been explored for fabricating hollow fiber membranes (HFMs) employed in liquid and gas separations since the 1970s. Some of its membranes have achieved industrial requirements under extremely harsh process environments (i.e., pH extremes, high temperatures, chlorine, organic solvents) due to its structural rigidity, robust mechanical stability, and outstanding chemical resistance. The development of high-performance industrially durable PBI HFMs is challenging owing to the complex interactions among the PBI polymer, solvents, and coagulant media during the non-solvent induced phase inversion process. State-of-the-art technologies have been developed to fabricate macrovoid-free PBI HFMs through non-solvent induced phase separation. Moreover, the chemically modified PBI membranes, PBI blended membranes and PBI composite membranes can not only improve the chemical resistance in organic solvents but also enhance the separation performance. The recently developed PBI gas separation HFMs also exhibit outstanding permselectivity and productivity exceeding the 2008 Robeson's upper bound for H2/CO2 separation at elevated temperatures (>200 °C). Therefore, this review aims to offer useful guidelines for researchers who are interested in PBI membranes for sustainable water and energy production. Both challenges and future opportunities of developing PBI-based HFMs will also be summarized and analyzed.
Fig. 1 Synthetic scheme of polybenzimidazole by a two-stage melt-solid polycondensation reaction.1 (3,3′-4,4′ Tetraaminodiphenyl is also referred to as 3,3′-diaminobenzidine (DAB)). |
In the beginning, PBI was explored as a thermally stable and non-flammable textile fiber to replace asbestos,2 and a high temperature matrix resin for aerospace and defence applications.8 Since the heterocyclic and amphoteric benzimidazole rings in PBI molecules could not only offer superior thermal stability but also be modified by strong acids to form proton conducting membranes,13 PBI has been extensively employed in fuel cells as polymer electrolyte membranes (PEMs) over the last 2 decades.14–16 Specifically, after being doped with phosphoric acid or sulfuric acid, the PBI/acid complex exhibits a higher proton conductivity, lower gas permeability, and durable operation.17–21 Wainright et al. first developed a PBI–phosphoric acid (PA) complex used in high-temperature fuel cells.17 Thus, extensive studies have been devoted to PBI syntheses, modifications, membrane formation and processing as high performance, low-cost PEMs used in high-temperature fuel cells.22–25 On the other hand, PBI and quaternized-PBI can serve as a framework in forming highly anion conducting anion exchange membranes (AEMs) with outstanding alkaline resistance.26–28 Comparing with conventional acidic fuel cells, AEM fuel cells have the most significant advantage of the much faster kinetics of the oxygen reduction reaction under alkaline operating conditions, which allows the use of non-precious metal catalysts (Ag, Ni, Co). The resultant AEM membranes can critically dominate the OH− transport while limiting the fuel crossover. The AEMs based on quaternized-PBI/GO and quaternized-PBI/PEI blends have also been adopted in electrodialysis (ED) and membrane capacitive deionization (MCDI) for water desalination.29,30
Since Loeb and Sourirajan synthesized asymmetric reverse osmosis (RO) membranes from cellulose acetate via the phase inversion approach in the late 1950s,31 polymeric membranes have become an attractive alternative to many energy-intensive separation processes, such as extraction, distillation, adsorption and chromatography. Systems based on pressure-driven polymer membranes become mature and accepted in many industrial separations due to their good performance, ease of scale-up, low energy consumption, environmental benignity, compact modular construction, and low operating costs compared with those thermal based systems.32–34 Successful isothermal operations of polymeric membranes with liquids have been realized to replace and/or combine with conventional separation processes. Because of the distinguished chemical resistance, mechanical and thermal stabilities, PBI membranes have been fabricated in the geometries of flat sheets and hollow fibers for many separation applications such as microfiltration (MF) and ultrafiltration (UF), RO, nanofiltration (NF), forward osmosis (FO), pervaporation (PV), organic solvent resistant nanofiltration (OSN), and gas separation, particularly employed in aggressive environments.
Comparing with flat-sheet membranes and tubular membranes, hollow fiber membranes (HFMs) possess many inherent advantages, such as a higher surface area to volume ratio, self-supporting characteristics and a smaller footprint although the fabrication of integrally skinned HFMs with less defects is a complicated and challenging process.34,35 This review aims to summarize (1) the developments of PBI materials including chemical modifications of PBI membranes and the variation of main chain structure during syntheses to augment their physicochemical properties and separation performance; (2) the research trends and recent development of macrovoid-free PBI HFMs fabricated by the non-solvent induced phase separation (NIPS); (3) the applications of PBI HFMs specially designed for water nanofiltration, solvent dehydration through pervaporation, organic solvent nanofiltration and H2/CO2 separation at elevated temperatures. Finally, the challenges and prospects of developing next-generation PBI materials and hollow fiber membranes will be discussed and analyzed.
Ignacz et al. presented a pioneering approach to ion-stabilize PBI and polymer of intrinsic microporosity (PIM-1) blended membranes via a simple HCl treatment without the use of covalent chemical crosslinking.46 The obtained robust PBI membranes were stable in polar aprotic solvents. The incorporation of PIM-1 into the PBI membranes improved the permeance up to 4 times, and simultaneously decreased the MWCO. Hardian et al. developed metal–polymer coordination (MPC) solvent-resistant NF membranes owing to the superior thermal and complexation ability of benzimidazole moieties.47 The formation of coordination bonds between the metal (copper(I) iodide, CuI) and PBI chains protected the membranes from dissolving in harsh organic solvents and improved the mechanical properties. The novel method to prepare MPC membranes provides a new route besides covalent cross-linking for the preparation of OSN membranes with tailored molecular sieving performance.
As reactive bifunctional alkyl halides, α,α′-dichloro-p-xylene (DCX), 1,4-dibromobutane (DBB) and α,α′-dibromo-p-xylene (DBX) can react with the –NH– groups of imidazole rings in PBI. Wang et al. tightened the PBI membrane structure using DCX and improved its salt rejections to separate cephalexin from aqueous solutions in NF and FO applications.49,50 Chen et al. used DCX to crosslink PBI flat sheet membranes for dye rejections in organic solvent environments.51 The DCX cross-linked PBI membranes exhibited strong tolerance (i.e., minimal swelling) in tetrahydrofuran (THF) and acetone, but they were still dissolvable in DMAc and NMP. Valtcheva et al. developed PBI OSN membranes through cross-linking modifications with the aid of DBX and DBB.52,53 The DBX-crosslinked PBI membrane displayed better stability in DMF and a higher solvent permeability than the DBB-crosslinked one. Both cross-linked PBI membranes were stable in extreme acidic and basic environments (pH 0 to 14). However, it was difficult to tailor the selectivity of the PBI membranes. Through the grafting modification of a long linear monoaminated polymer on the DBX-crosslinked PBI membranes, solvent stable spiral wound modules were scaled up and showed potential for industrial applications.54
Tashvigh et al. used DBX and hyperbranched polyethylenimine (HPEI) to double cross-link PBI/sulfonated polyphenylsulfone (sPPSU) blend membranes.55 The addition of sPPSU and the double cross-linking process resulted in membranes with a higher solvent flux. The membranes had smaller pores but the permeance was not affected significantly. Tashvigh & Chung also fabricated thin film composite (TFC) membranes by forming an ultrathin and strong HPEI-DBX selective layer on top of the DBX crosslinked PBI substrate.56 The resultant membranes not only showed good chemical stability in DMAc at 50 °C but also had an MWCO of ∼350 g mol−1 with ethanol, acetone, THF and toluene permeances of 4.5, 14.0, 4.0 and 1.0 L m−2 h−1 bar−1, respectively. Recent achievements from Prof. Szekely's group were realized through ionically crosslinking PBI with difunctional organic acids in water to improve membrane properties. The reversible nature of the PBI-based membranes enabled the successful recovery of the pristine PBI by treatment under mild basic conditions.43
Farahani and Chung developed a facile crosslinking approach to fabricate high-flux OSN PBI membranes by cross-linking the PBI membrane with trimesoyl chloride (TMC) in 2-methyl tetrahydrofuran (2-MeTHF) at room temperature.57 The resultant PBI membrane had a high pure n-hexane permeance of 80.8 L m−2 h−1 bar−1 and a rejection of 90.4% to tetracycline. It also displayed stable performance in ethanol, acetone, isopropanol, and acetonitrile. As illustrated in Fig. 3, Fei et al. synthesized hydroxylated PBI–OH by the N-benzylation of PBI with 4-(chloromethyl)benzyl alcohol, blended it with graphene oxide (GO) and then covalently cross-linked the PBI/GO films with diisocyanate as mixed matrix membranes (MMMs).58 It was found that the anchored GO could stabilize the polymer matrix through robust π–π interactions with the modified PBI polymer chains.59 The PBI/GO membranes not only showed high permeances in high polarity solvents but also had a high rejection > 93% for a solute with a molecular weight of 420 g mol−1 in both polar and nonpolar solvents, such as acetone, THF, acetonitrile (MeCN), dichloromethane (DCM), and DMF. Zhao et al. fabricated robust PBI composite membranes through encapsulating a dopamine monomer in the PBI membrane matrix by NIPS, followed by in situ polymerization of dopamine initiated with NaIO4 to form an interpenetrating polymer network (IPN),60 as shown in Fig. 4. Although both FTIR and solid-state NMR analyses did not detect the occurrence of covalent cross-linking modifications, the membrane displayed solvent stability in seven polar aprotic solvents up to 100 °C due to the combined effects from the strong secondary interaction between PBI and polydopamine (PDA), and the formation of IPN. A permeance up to 12 L m−2 h−1 bar−1 in DMF was obtained with a MWCO of 190–850 g mol−1. PDA can also be used as a functional layer for an additional coating or as a selective layer by various crosslinking approaches. Fei et al. reported a pioneering study by using an oxidant-promoted biophenol coating as a versatile, reproducible, and easily scalable method to finely tailor the separation performance of PBI OSN membranes.61 Kim et al. developed a robust and tight PBI-based OSN membranes through reinforcing the active layer with an ultrathin PDA coating followed by the simultaneous co-crosslinking of the PDA-coated PBI membranes.62 The PDA layer can effectively improve the pristine PBI membrane performance by reducing the overall pore size and filling the defects at the PBI membrane surface. PDA coated PBI/GO composite membranes for oil-in-water emulsion separation demonstrated promising long-term antifouling and antimicrobial properties.63
Fig. 3 Reaction scheme showing the N-benzylation of polybenzimidazole and the diisocyanate-based (A) cross-linking of hydroxylated polybenzimidazole chains, (B) anchoring of GO sheets, and (C) cross-linking of GO sheets. Reproduced with permission from ref. 58, copyright 2018, ACS Publications. |
Fig. 4 Schematic overview of the membrane fabrication methodology for in situ polymerized polydopamine (PDA)/polybenzimidazole (PBI) interpenetrating polymer network (IPN): (A) casting a dope solution comprising PBI and dopamine monomers, (B) phase inversion in water, (C) immersing the membrane in an aqueous NaIO4 initiator, and (D) in situ polymerization of dopamine in a tris buffer solution. (E) IPN of linear PBI and branched PDA. (F) Molecular-level interactions between PBI and PDA polymers. Reproduced with permission from ref. 60, copyright 2019, ACS Publications. |
Two-dimensional (2D) materials such as graphene oxides (GOs), MoS2, and MXene can be made into a laminar membrane through stacking 2D single layers with sub-nanometer channels that serve as molecular sieves to separate small gas molecules (i.e., H2 or He) from large gas molecules (i.e., N2, CO2, and CH4).68–70 Jin et al. developed a cross-linked PBI-triglycidylisocyanurate (TGIC) and 2-D sulfonated graphene (SG) composite membrane with a thickness of 132 μm.70 It could separate H2 from CO2 based on the mixed proton–electron conducting mechanism, in which protons diffused by hopping along the cross-linking sites between the sulfonic groups of SG and the pyrrole rings of PBI, while electrons were transported via the highly electron conductive SG, as shown in Fig. 5. By adding SG, the membrane became more compact due to the smaller interlayer spacing and swelling ratio. The PBI–TGIC/SG membrane can separate H2 from the H2/CO2 mixture (50:50 v/v)) with 99.99% selectivity (infinite) and a high permeability of up to 1676 barrer at 300 °C due to the mixed conducting property of the composite membrane.
Fig. 5 Schematic diagram of the mixed conducting mechanism in the MPEC PBI-TGIC/SG membrane. Reproduced with permission from ref. 70, copyright 2021, the Royal Society of Chemistry. |
Fig. 6 Representation of PBI structural packing: π–π stacking and hydrogen bonding. Reproduced with permission from ref. 76, copyright 2016, Elsevier. |
Various molecular designs and modifications have been proposed to improve the gas permeability of PBIs including optimization of the main chain structure, N-substitution modification, as well as aforementioned chemical cross-linking modifications. It is well known that systematically alternating the backbone structure of a polymer with inhibited chain packing and mobility tends to increase permeability while maintaining or increasing selectivity.78,79 Therefore, by introducing bulky groups into the PBI main chains, one can increase the distance between molecular chains and enlarge the free volume without seriously losing the chain rigidity. As listed in Table 1, structurally modified PBI materials were obtained by varying the acid moiety during PBI syntheses via solution polymerization using either DAB or substituted aromatic dicarboxylic acids. The optimized PBI materials had a reduced chain packing density, but slightly decreased thermal stability.73,74,80 In addition, the introduction of (1) tert-butyl groups in PBI–BuI and (2) hexafluoroisopropylidene groups in PBI–HFA improved solubility in pyridine and NMP, while the incorporation of bromine in PBI–BrT and PBI–DBrT enhanced their solvent solubility. However, the solubility of PBI-T was reduced due to the improvements of chain rigidity and symmetry, and intermolecular attraction. All the derived PBIs were amorphous in nature and exhibited high degradation temperatures (>400 °C).
PBI polymer abbreviation | Dicarboxylic acid, HOOC–R–COOH | R Chemical structure | Polymerization solvent, T (°C) | IV (dL g−1) | Ref. |
---|---|---|---|---|---|
a Polybenzimidazoles were synthesized by a solution polycondensation method based on 3,3′-diaminobenzidine (DAB) and dicarboxylic acid. b Polybenzimidazoles were synthesized by a solution polycondensation method based on tetraaminodiphenylsulfone (TADPS) and dicarboxylic acid. c PPA, polyphosphoric acid. | |||||
PBI-I | Isophthalic acid (IPA) | PPAc, 200 °C | 1.4 | Kumbharkar et al. 2006,74 2009 (ref. 80) | |
PBI-T | Terephthalic acid (TPA) | PPAc, 200 °C | 1.8 | Kumbharkar et al. 2009 (ref. 80) | |
PBI-Bul | 5-tert-Butylisophthalic (Bul) | PPAc, 200 °C | 1.3 | Kumbharkar et al. 2006,74 2009 (ref. 80) | |
PBI-HFA | 4,4′-(Hexafluoroisopropylidene)bis (benzoic acid) (HFA) | PPAc, 200 °C | 1.4 | Kumbharkar et al. 2006,74 2009 (ref. 80) | |
PBI-BRT | 2-Bromoterephthalic acid (BrTPA) | PPAc, 200 °C | 1.3 | Kumbharkar et al. 2009 (ref. 80) | |
PBI-DBRT | 2,5-Dibromoterephthalic acid (DBrTPA) | PPAc, 200 °C | 1.3 | Kumbharkar et al. 2009 (ref. 80) | |
PBI-2,6Py | 2,6-Pyridinedicarboxylic acid (PyA) | PPAc, 200 °C | 0.9 | Kumbharkar et al. 2009 (ref. 80) | |
6F-PBI | 2,2-Bis(4-carboxyphenyl)-hexafluoropropane | PPAc, 220 °C | 1.4 | Li et al. 2014 (ref. 73) | |
PBI-PFCB | 4,4′-((1,2,3,3,4,4-Hexafluorocyclo-butane-1,2-diyl) bis(oxy))dibenzoic acid | Eaton's reagent, 140 °C | 0.73 | Li et al. 2014 (ref. 73) | |
PBI-BTBP | 2,2′-Bis(trifluoromethyl)benzidine | Eaton's reagent, 140 °C | 1.6 | Li et al. 2014 (ref. 73) | |
PBI-phenylindane | 1,1,3-Trimethyl-3-phenylindan-4′,5-dicarboxylic acid | PPA, 195 °C | 0.8 | Li et al. 2014 (ref. 73) | |
TADPS-OBA | 4,4′-Oxybis(benzoic acid) (OBA) | Eaton's reagent, 140 °C | — | Borjigin et al. 2015 (ref. 85) | |
Stevens et al. 2020 (ref. 72) | |||||
TADPS-TPA | Terephthalic acid (TPA) | Eaton's reagent, 140 °C | — | Borjigin et al. 2015 (ref. 85) | |
Stevens et al. 2020 (ref. 72) | |||||
TADPS-IPA | Isophthalic acid (IPA) | Eaton's reagent, 140 °C | — | Borjigin et al. 2015 (ref. 85) | |
Stevens et al. 2020 (ref. 72) |
As shown in Fig. 7, Li et al. synthesized four PBI derivatives containing bent and rigid configurations that possessed bulky side groups and could frustrate close chain packing.73 Comparing with commercial m-PBI, the structurally modified PBIs had higher molecular weights, slightly decreased thermal stabilities, and enhanced organo-solubilities. Table 2 confirms that the introduction of bulky, flexible and frustrated functional groups into the PBI backbone effectively produced new PBIs with much higher H2 permeability. However, these PBI derivatives showed a lower H2/CO2 selectivity range of 5–7 than that of m-PBI because of the trade-off relationship between gas permeability and selectivity. As shown in Fig. 8, all PBI-based membranes exhibit higher gas separation performance than the 2008 Robeson's upper bound prediction at 250 °C (ref. 65) and are promising materials for H2 separation from syngas at high temperatures. Among these polymers, the 6F–PBI membrane had an interesting relationship between CO2 permeability and temperature because its permeability remained nearly constant from near-ambient temperature to 250 °C.73 This unique phenomenon resulted from the combined effects of temperature-dependent solubility and diffusivity. At low temperatures, there was a strong CO2–polymer interaction due to the presence of highly electronegative 6F groups, while at high temperatures, CO2 solubility decreased rapidly but diffusivity increased quickly. This led to an almost constant CO2 permeability over the evaluated temperature range. Owing to the high H2 permeance and thermal resistance at elevated temperatures, 6F–PBI or PBI–HFA has been used to seal defects on the selective surface of PBI hollow fiber membranes to mitigate the influence of pin–hole defects,81,82 similar to the role of commonly adopted silicone rubber. Since 6F–PBI has a high H2 permeability due to the presence of highly disrupted and loosely packed hexafluoroisopropylidene diphenyl groups while m-PBI has a high H2 selectivity owing to the tightly packed phenylene group, Singh et al. synthesized 6F–PBI/m-PBI copolymers with a tailorable permeability and selectivity, and a high inherent viscosity.83 The H2/CO2 separation performance of these copolymers surpassed the 2008 Robeson's upper bound at 250 °C.65
Fig. 7 Synthetic schemes of PBI derivatives (a. m-PBI; b. 6F-PBI, PFCB-PBI, BTBP-PBI, and phenylindane-PBI). Reproduced with permission from ref. 73, copyright 2014, Elsevier. |
PBI membrane | Feed gas | ΔP | T (°C) | H2 permeance (GPU) | H2 permeability (Barrer) | H2/CO2 selectivity | Ref. |
---|---|---|---|---|---|---|---|
a 1 Barrer = 1 × 10−10 cm3 (STP) cm cm−2 s−1 cmHg−1, 1 GPU = 1 × 10−6 cm3 (STP) cm−2 s−1 cmHg−1 = 7.50 × 10−12 m s−1 Pa−1. b Estimated from their figures.73 c The m-PBI membrane was fabricated from a Celarole® S10 PBI solution. | |||||||
PBI–I | Pure | 2.1 × 106 Pa (300 psia) | 35 | — | 0.63 | 3.8 | Kumbharkar et al. 2006,74 2009 (ref. 80) |
PBI–T | 0.16 | — | |||||
PBI–BuI | 10.66 | 5.58 | |||||
PBI–HFA | 12.15 | 4.18 | |||||
PBI–BrT | 0.38 | — | |||||
PBI–DBrT | 1.89 | — | |||||
PBI–2,6Py | 1.38 | — | |||||
m-PBI | Pure | 3.4 × 105 Pa (50 psia) | 250 | 3.6 | 76.81 | 23.03 | Li et al. 2014 (ref. 73) |
6F-PBI | 162.1 | 997.2 | 5.174 | ||||
BTBP-PBI | 89.07 | 710.4 | 7.111 | ||||
Phenylindane-PBI | 24.55 | 480.6 | 6.522 | ||||
PFCB-PBI | 22.55 | 323.1 | 6.604 | ||||
TADPS-OBA | Pure | 1.0 × 106 Pa (10.0 atm) | 35 | — | 5.7 ± 0.2 | 10 | Borjigin et al. 2015 (ref. 84) |
TADPS-TPA | 5.5 ± 0.3 | 20 | |||||
TADPS-IPA | 3.6 ± 0.3 | 32 | |||||
m-PBI | Pure | 3.0 × 105 Pa (3.0 atm) | 190 | — | 22.1 ± 0.6 | 23.3 ± 0.9 | Stevens et al. 2020 (ref. 72) |
TADPS-OBA | 38 ± 1 | 18 ± 2 | |||||
TADPS-TPA | 31 ± 3 | 24.6 ± 0.9 | |||||
TADPS-IPA | 30.1 ± 0.8 | 9.7 ± 0.4 | |||||
m-PBIb | Pure | 1.4 × 105 Pa (20 psia) | 43 | — | 4.0 | 16.8 | Li et al. 2014 (ref. 73) |
m-PBIc | Pure | 1.1 × 106 Pa (11.0 atm) | 35 | — | 2.0 ± 0.1 | 12 ± 1 | Zhu et al. 2017 (ref. 64) |
m-PBI | Pure | 2.7 × 105 Pa (2000 torr) | 35 | — | 1.11 ± 0.03 | 11.1 ± 1.1 | Panapitiya et al. 2015 (ref. 71) |
m-PBI | Pure | 3.0 × 105 Pa (3.0 atm) | 35 | — | 2.4 ± 0.1 | 24 ± 1 | Stevens et al.2020 (ref. 72) |
Fig. 8 Robeson plot comparing the PBI derivative membranes with other polymeric membranes tested for the H2/CO2 separation. Reproduced with permission from ref. 73, copyright 2014, Elsevier. |
Fig. 9 shows another type of highly permeable thermally rearranged PBI (TR-PBI) membranes with microporous characteristics (i.e., high free volume fraction and large average d-space) by the scheme from polypyrrolone (PPL) via the ring-opening reaction in an alkaline solution, and a thermal treatment followed by decarboxylation at 450 °C.84 The TR-PBI membranes treated at 450 °C had a H2 permeability of 1779 barrer and an ideal H2/CO2 selectivity of 1.1 at 25 °C. Although the H2/CO2 selectivity was low, it could be improved by increasing the feed temperature since the CO2 permeability would drop significantly due to the decrease in CO2 solubility at higher temperatures of more than 200 °C.
Fig. 9 Synthesis route to microporous polybenzimidazole (TR-PBI) from polypyrrolone (PPL) using a thermal rearrangement concept. Reproduced with permission from ref. 84, copyright 2010, Elsevier. |
Borjigin et al. synthesized PBIs containing sulfonyl groups and fabricated them as high temperature membranes for H2/CO2 separation.85 As illustrated in Fig. 10, the rigid 3,3-diamine monomer was substituted by the monomer of 3,3′,4,4′-tetraaminodiphenylsulfone (TADPS). The flexible and kinked sulfonyl linkage in the main chain structure not only enhanced the PBI solubility but also inhibited the chain packing and interchain interactions.72 As a result, these novel PBIs had enhanced Tg and solubilities in dipolar aprotic solvents that facilitated the solution casting of thin and defect-free membranes. Table 2 also summarizes their gas separation properties for H2/CO2 separation at 35 °C.
Fig. 10 Synthesis of polybenzimidazole using Eaton's reagent as a solvent.72 PPMA (Eaton's reagent): phosphorus pentoxide/methanesulfonic acid. |
N-substituted polybenzimidazoles were also synthesized by using selective bulky or flexible side groups in order to break the intermolecular H-bonding, disrupt chain packing and increase the gas permeability.86 Although both the Tg and degradation temperature of N-substituted PBIs became lower owing to the increase in chain flexibility, the gas permeability increased while the gas selectivity declined. Similarly, the gas sorption capability increased because of the loose chain packing and weak H-bonding. In addition, the solubility in solvents of chloroform and trichloroethylene was enhanced.86 As a result, N-substituted PBIs have gas separation properties more suitable for other gas pairs rather than for H2/CO2 separation.87
As a class of porous organic frameworks (POFs), benzimidazole-linked polymers (BILPs) have been synthesized by the condensation reaction between aryl-o-diamines and aldehydes in DMF to form amorphous powders with network structures.88,89 The resultant BILPs were insoluble in solvents and had outstanding thermal and chemical stabilities, as well as high CO2 uptakes. They may be a good candidate for CO2 capture, storage as well as other industrial separations. Shan et al. prepared defect-free BILP membranes by using the interfacial polymerization method and the resultant membrane exhibited excellent separation performance with a permeance of 24 GPU and H2/CO2 selectivity of 40 at 150 °C using an equimolar H2/CO2 mixture as the feed at 1 bar.90 Wang et al. followed the same approach and synthesized BILP membranes suitable for He/CH4 separation.91 Both membranes have separation performance surpassing the 2008 Robeson upper bounds. So far, BILP-based PBI membranes have not received much attention especially on the fabrication and applications of their HFMs.
The NIPS process can be qualitatively illustrated by a triangle phase diagram which describes the thermodynamic interactions among the polymer, solvents, and non-solvents. The binodal curve divides the triangle into two regions, namely, a single-phase region where all components are miscible and a two-phase region where the homogeneous solution separates into a polymer rich phase and a polymer lean phase,93,94 as shown in Fig. 11. During the phase inversion, the nascent membrane starts to cross the binodal curve, its composition is divided into two phases connected by a tie line. The polymer-rich and polymer-lean phases would eventually develop into the polymer matrix and pores, respectively. Ideally, the final morphology of as-cast flat-sheet membranes is mainly related to the initial casting composition, binodal curve position, and precipitation path if no external forces or factors are applied. Generally, kinetics will affect the precipitation path for a given polymeric solution, whereas thermodynamics controls the position of binodal points during the phase inversion.93–96
During the spinning of a hollow fiber membrane (HFM), a polymer solution and a bore fluid are extruded through a spinneret simultaneously and a nascent hollow fiber begins to form and then enters the coagulation bath where solvents and nonsolvents are fully exchanged, as shown in Fig. 12. The bore fluid that occupies the lumen space can be simply removed during the solvent exchange and drying steps. Different from flat-sheet membranes, the fabrication of hollow fibers involves two coagulants (i.e., internal and external coagulants) which influences the formation of the inner and outer surfaces, respectively. Depending on the two coagulants' chemistry, solubility parameters and other factors, they may determine where the selective layer is formed. For example, the evaporation of volatile components in the air gap region can cause the outermost surface of the nascent hollow fiber to approach a vitrified state, thus a dense skin is formed on the outer layer of the hollow fiber. Once the nascent hollow fiber enters the coagulant bath, both inner and outer coagulants would diffuse into the hollow fiber and induce a porous substrate that provides the overall mechanical strength. In this way, a desirable integrally skinned asymmetric hollow fiber membrane with a dense layer on top of a porous substructure is formed. Spinning parameters have important influences on the phase inversion process, including dope and bore fluid compositions, dope viscosity, air gap distance, extrusion rates of the dope and bore fluid, and take-up speed. The manufacturing process of HFMs in large scale production is shown in Fig. 13.
Fig. 12 Schematic of the enlarged regions inside and outside of the spinneret and the formation of a nascent hollow fiber membrane via a NIPS process. |
Hollow fiber membrane modules have several advantages over both tubular modules and spiral-wound modules made of flat-sheet membranes, including a higher ratio of surface to volume and a much smaller footprint.35,97,98 In addition, spiral wound modules require (1) a higher energy input due to the pressure drop along the spacer-filled channels and (2) extensive pre-treatment of feed solutions to reduce fouling.99 In contrast, HFMs need less pre-treatment and operation maintenance while keeping a relatively high packing density. Due to the advances in multi-filament spinning capability, modern HFM fabrication systems have achieved exceedingly high productivity.100 They can offer module surface area-to-volume ratios approaching 1000–10000 m2 m−3.35,101,102 Usually, a thick dense-selective layer in hollow fiber membranes may offset some of the surface area advantage of the fiber configuration, but it is feasible to increase the module productivity (i.e., surface area) per unit volume by an order of magnitude.33 In addition, HFMs can withstand a high transmembrane pressure difference (up to 70 bar) while the manufacturing cost is 5–20 times lower than those of equivalent membranes used for spiral wound modules in large-scale gas separation applications.97
It is well known that macrovoids may be formed in polymeric membranes via NIPS if the nonsolvent/solvent exchange is very rapid while the rapid solvent exchange is necessary to create an ultrathin dense-selective skin on the membrane surface. In general, macrovoids with finger-like and tear-drop shapes in asymmetric HFMs are considered as weak mechanical points which generate high stress areas and cause fiber failure under vibrations in membrane bioreactors (MBRs) or high pressures for gas separation especially at high temperatures.35,95,96,108 When the operation temperature is close to the Tg of the polymer, the enhanced chain mobility leads to increasing the susceptibility of structural collapse at these defect locations under high transmembrane pressures.109 In addition, the presence of macrovoids near the outer surface of HFMs often results in a defective selective layer.82 The technology to develop macrovoid-free HFMs is crucial for the rapidly growing membrane applications.
The origin of macrovoids is one of the debatable subjects among membrane scientists in the last 5 decades. Early researchers believed it could arise from instantaneous liquid–liquid demixing and the nucleation of droplets in the lean polymer phase due to the diffusion-driven mechanism,110–112 while others thought it could start from local mechanical instability, surface rupture and non-solvent intrusion, followed by rapid nucleation of droplets in the lean polymer phase.113,114 Other mechanisms such as Marangoni effects,115 osmosis pressure116 and solutocapillary convection mechanism117–119 had also been proposed. The solutocapillary convection mechanism consisted of diffusion and Marangoni force generated by local surface tension gradients. Clearly, macrovoid formation may involve multiple mechanisms taking effect simultaneously due to the existence of large differences in viscosity and concentration gradients between the two phases.35,96 Today, two mechanisms as well as their combined mechanism are mostly accepted for macrovoid formation: (1) the diffusion mechanism with the aid of solutocapillary convection, and (2) local surface instability, skin rupture and non-solvent intrusion.
Several methods have been proposed to suppress macrovoid formation, such as: (1) increasing polymer concentrations or dope viscosity120 or adding components with high viscosity,121,122 (2) inducing delayed demixing or gelation,116,123 (3) adding surfactants in dopes,124 (4) decreasing dope temperature125 or increasing temperature in the coagulation bath,126 (5) spinning at high shear rates or high elongational rates.120,127,128 Although increasing the dope viscosity by the aforementioned methods is an effective means to lower non-solvent intrusion and minimize macrovoid formation, it often leads to a thick dense-selective layer.96,129 One must also choose a suitable solvent–nonsolvent system during the phase inversion process to produce membranes with the desirable morphology, mechanical properties and separation performance.
Solubility parameter has been extensively used to predict the solubility of polymers in solvents. The Hanson solubility parameter (δ) of a material is determined by the group contributions from its structural elements based on dispersion forces (referred to as δd), polar interactions (δp) and hydrogen bonding (δh).130 The total solubility parameter (δT) of a polymer is a sum of these three contributions, as written in eqn (1). When dissolving a polymer in a solvent, the difference in their solubility parameters, ΔδS–P, can be calculated from eqn (2). The combined parameter, δv, is defined as eqn (3).131
δT = (δd2 + δp2 + δh2)1/2 | (1) |
ΔδS–P = [(δd,S − δd,P)2 + (δp,S − δp,P)2 + (δh,S − δh,P)2]1/2 | (2) |
δv = (δd2 + δp2)1/2 | (3) |
Table 3 lists the solubility parameters of PBI, some solvents and non-solvents. For a given polymer, one can determine the “solubility circle” associated with the polymer and solvents according to the ΔδS–P values. When the ΔδS–P value is less than 5, the solvents inside this circle are considered as “good” solvents that will dissolve or swell the polymer.132 Usually, the combined parameter δv is plotted against δh to compare various polymer/solvent systems. As illustrated in Fig. 14, DMAc, NMP and acetone, are good solvents for PBI although PBI is insoluble in acetone, while MeCN, ethylene glycol, and THF are non-solvents (NS).
Polymer or Solvent | δ p (MPa1/2) | δ d (MPa1/2) | δ h (MPa1/2) | δ P or δS (MPa1/2) | δ S-P (MPa1/2) |
---|---|---|---|---|---|
PBI | 8.7 | 17.3 | 8.9 | 21.3 | — |
DMAc | 11.5 | 16.8 | 10.2 | 22.8 | 3.1 |
NMP | 12.3 | 18.0 | 7.2 | 23.0 | 4.0 |
DMF | 13.7 | 17.4 | 11.3 | 24.9 | 5.5 |
THF | 16.8 | 5.7 | 8.0 | 19.4 | 14.2 |
MeCN | 18.0 | 15.3 | 6.1 | 24.4 | 9.9 |
Acetone | 10.4 | 15.5 | 6.9 | 20.0 | 3.2 |
Toluene | 18.0 | 1.4 | 2.0 | 18.2 | 19.7 |
EG | 17.0 | 11.0 | 26.0 | 32.4 | 20.0 |
Water | 16.0 | 15.5 | 42.3 | 47.8 | 34.2 |
Fig. 14 Solubility parameter plot for PBI and organic solvents. δd, δp, and δh (Hansen parameters) are the contribution of dispersive force, polar force and hydrogen bonding, respectively. The green circle represents a solubility parameter difference between PBI and organic solvent of less than 5.82 |
The solubility parameter difference between the solvent and non-solvent will influence the solvent exchange rate and alter the polymer solubility in the transient polymer/solvent/non-solvent mixture during the non-equilibrium state of the phase inversion process. Generally, a closer solubility parameter between the polymer solution and nonsolvent would result in a delayed demixing, thereby obtaining a more porous membrane structure without macrovoids. In contrast, if they have a larger difference in solubility parameter, it may result in an asymmetric membrane with a dense nonporous top layer with macrovoids due to the instantaneous dimixing.
A breakthrough was made by Singh et al. who added acetonitrile in diluted PBI solutions, discovered its effectiveness to augment the dope viscosity and produced dry-jet wet-spun PBI HFMs with a desirable morphology; namely, an outer dense-selective layer and a macrovoid-free porous substrate.82 Acetonitrile (MeCN) was chosen because it (1) is a weak solvent to PBI, (2) is a low boiling solvent (82 °C), (3) is highly soluble in water, and (4) has smaller MW than DMAc (41.05 vs. 87.12 g mol−1). As a result, it increased the PBI dope viscosity due to the enhanced inter- and intra-molecular frictions among PBI chains and thus minimized the non-solvent intrusion during phase inversion, while its characteristics of high solubility in water, small MW and size, and low boiling point facilitated (1) the solvent/nonsolvent exchange in a wet-spinning process or (2) the solvent evaporation in a dry-jet wet-spinning process, thus forming a thin outer-selective layer. In addition, the authors adopted a PBI/DMAc/MeCN spinning solution very near to the precipitation point. Therefore, a small variation of dope composition due to the solvent/nonsolvent exchange could result in a uniform precipitation across the membrane. The obtained PBI HFMs have a bi-continuous sponge-like substructure that not only improved the overall mechanical strength of HFMs but also minimized the gas transport resistance. By manipulating the PBI HFM spinning parameters, the thickness of the dense-selective layer could be finely tuned between 200 and 2000 nm. The resultant PBI HFMs coated with 6F-PBI (i.e., as a defect sealant) had a H2 permeance one to two orders of magnitude higher than those reported by Kumbharkar et al.81 and Dahe et al.132 with a comparable H2/CO2 selectivity.
Fig. 15 Schematic diagram of spinneret for dual-layer hollow fiber spinning. Reproduced with permission from ref. 134, copyright 2002, Elsevier. |
The most important issues with dual-layer HFMs are (1) delamination and (2) poor adhesion between the two polymeric layers. Delamination is often observed between the two layers due to their different shrinkage rates during phase inversion.134 To overcome it, in addition to adjusting the spinning conditions, one can incorporate nanoparticles into the inner layer to lower its shrinkage rate or use an indented dual-layer spinneret to premix and enhance molecular diffusion between the two layers.136 To improve the interfacial adhesion, the miscibility of the two polymers must be considered. A good adhesion can be achieved if the two polymers are partially miscible.144 In addition, the incorporation of a small number of nanoparticles into the selective layer appears to be effective to achieve a good interfacial adhesion between the two layers.139,148 One of the reasons arises from the fact that the addition of nanoparticles into the selective-layer dope may increase its viscosity, retard nonsolvent intrusion and mitigate the formation of large voids (i.e., weak points) between the two layers.
A seamless interface is essential for the long-term structural integrity and separation performance of HFMs, especially at high pressures. PBI as the selective layer has been made into dual-layer HFMs through the co-extrusion process with other polymers. Delamination-free PBI/PAN (i.e., PBI/polyacrylonitrile) dual-layer HFMs,139 PBI/P84 (i.e., PBI/co-polyimide, BTDA-TDI/MDI),141,142,145 PBI/PEI (i.e., PBI/polyetherimide),106,149,150 and PBI/PES (i.e., PBI/polyethersulfone)151,152 have been fabricated and used for various membrane separations.
Operating temp. (°C) | Testing time (hr) | Final flux of CA membranes L m−1 h−1 (gal ft−2 d−1) | Final flux of PBI membranes L m−1 h−1 (gal ft−2 d−1) |
---|---|---|---|
70 | 5 | 20.4(12) | 27.2(16) |
120 | 5 | 34(20) | 28.9(17) |
167 | 20 | 8.5(5) | 32.3(19) |
194 | 5 | 0(0) | 42.5(25) |
Recently, both Wang et al.178 and Wales et al.179 fabricated PBI RO HFMs without finger-like macrovoids from PBI/DMAc/PVP/IPA dopes using MeOH/IPA mixtures as the internal and external coagulants. Fig. 16 shows one of their morphologies.178 The PBI hollow fiber membranes exhibited good separation performance with a pure water permeability of 0.07 L m−2 h−1 bar−1 and a NaCl rejection of 99.0% after being treated with a 1000 ppm NaClO solution for 1 h. These performances were comparable to the commercial CTA RO HFMs produced by Toyobo Co. Ltd.178 The PBI HFM demonstrated the stable operation of a single-stage RO system for treating concentrated flue gas desulfurization (FGD) wastewater with a salt rejection of 97%.179 However, since polyamide-based thin-film composite (TFC) membranes invented in the 1980s180,181via in situ interfacial polymerization have impressively high RO performance and currently dominate the market of seawater desalination, the importance of PBI RO membranes has been significantly reduced.
Fig. 16 Typical morphology of a polybenzimidazole RO hollow fiber membrane.Reproduced with permission from ref. 178, copyright 2018, MDPI. |
Chemically, PBI is a weakly basic polymer. It has a pKa value of 5.5 in the protonated form14 due to the fact that its heterocyclic imidazole group has two nitrogen atoms. The one attached to the H atom can be a hydrogen bond donor while the nitrogen with the lone pair is more likely to be a proton acceptor.188 PBI may become self-charged in aqueous solutions since the adjacent benzene ring delocalizes the proton of the imidazole group. The self-charging feature can be used to directly develop PBI NF HFMs without additional modifications. Moreover, PBI-based NF membranes can overcome one major shortcoming of polyamide-based TFC NF membranes because the latter is vulnerable to chlorine attack during the chemical cleaning and disinfectant processes for water and wastewater treatment.99
Many research efforts have been devoted, since the early 2000s, to the fabrication of single- and dual-layer PBI-based NF HFMs through the NIPS process. Wang & Chung investigated the effects of bore fluid on the morphology and separation performance of PBI HFMs.107,189 By using a mixture of DMAc and ethylene glycol as the bore fluid, the resultant PBI HFMs have no macrovoids in the inner substrate, as illustrated in Fig. 17. Therefore, the PBI HFMs could withstand a high operation pressure up to 30 bar. The asymmetric PBI NF HFMs had a PWP of 1.86 L m−2 h−1 bar−1, a mean effective pore size of 0.348 nm in radius and a narrow pore size distribution. They could effectively segregate ions from salt mixtures because they had high rejections to divalent cations and anions while low rejections to monovalent ions. Clearly, the PBI NF HFMs can (1) remove heavy metals from wastewater and (2) separate chromate and sulfate ions from brines to facilitate the chlor-alkali process even under a high pH up to 14.189,190 To further reduce the material cost and transport resistance but retain the high rejection characteristics, dual-layer PBI/PES NF HFMs were also developed.191 The thickness of the PBI layer could be reduced to around 6 μm without compromising the separation performance. Therefore, both single- and dual-layer PBI NF HFMs have great potential to effectively remove heavy metal ions in various industries.
Fig. 17 Morphology of an asymmetric PBI nanofiltration hollow fiber membrane.Reproduced with permission from ref. 189, copyright 2006, Elsevier. |
PBI based HFMs have also been explored in (1) forward osmosis (FO) for water reclamation151,192–194 and protein concentration,152 (2) pressure-retarded osmosis process (PRO) for power generation139,195,196 and (3) organic solvent nanofiltration (OSN). Among them, PBI membranes for OSN have received most attention because most FO and PRO processes do not involve harsh environmental and testing conditions.
Although some lab-scale OSN HFMs have been made from chemically resistant or cross-linkable polymers, such as polyacrylonitrile (PAN),206,207 polyphenylsulfone (PPSU),208 polyimides/polyamides (e.g. P84,209 Torlon,210,211), there are still no commercially available OSN HFMs for industrial applications. Since PBI already has limited dissolution in common solvents, the chemically crosslinked PBI should possess much higher chemical stability against plasticization and swelling in polar solvents. Moreover, different from the crosslinking modifications of PAN and polyimide membranes, the PBI backbone structure remains unchanged and strong after the modifications, making it a potential polymer to fabricate integrally skinned asymmetric OSN HFMs.
A dual-layer OSN HFM was synthesized by a coextrusion-crosslinking approach using PBI as the outer selective layer and in situ HPEI crosslinked P84 as the inner substrate layer.145 The composite OSN HFM showed a rejection of >99% to methylene blue (MW: 319.85 g mol−1) and good solvent permeances in water, methanol and MeCN. The chemical stability and selectivity of PBI membranes were largely improved in organic solvents. Tashvigh et al. synthesized acid-doped PBI HFMs after immersing them in a 2.0 wt% H2SO4/isopropanol solution.42 The modified PBI membranes displayed remarkable stability in DMAc and DMF, fair stability in DMSO but poor stability in NMP due to the H-bonding between NMP and PBI which would weaken the performance of acid-doped PBI membranes. Therefore, doping PBI membranes with a strong acid might cause a leaching issue. By using a green cross-linking process, Zhao et al. modified PBI HFMs with a K2S2O8 aqueous solution at 35 °C.45 The resultant PBI membranes not only had greater stability in harsh solvents such as NMP, DMF and DMSO, but also showed better mechanical properties due to the newly formed N–N covalent bonds among different PBI chains. Wang et al. adopted a double modification strategy to fabricate integrally skinned PBI-DBX-SCA8 HFMs by combining DBX covalent crosslinking and 4-sulfocalix[8]arene (SCA8) ionic impregnation.212 Synergistical improvements in chemical stability, molecular sieving ability and mechanical strength were observed. The PBI HFMs showed broad tolerance to polar, non-polar and aprotic polar solvents and had a controllable molecular-level separation ability. One-inch PBI HFM modules were also fabricated to demonstrate their long-term performance for solvent recovery from various acetone/oil mixtures.
Both single- and dual-layer PBI HFMs have been fabricated for pervaporation dehydration of organic solvents, such as ethylene glycol, acetone, ethyl acetate, phenol, alcohol, as well as organic–organic separation. Water can preferentially permeate across PBI membranes because it has a stronger affinity with PBI molecules and a smaller molecular size than most organic solvents. Wang et al. prepared single-layer PBI HFMs for the dehydration of ethylene glycol which showed much better separation performance in both permeance and separation factor than the PBI flat-sheet membranes.106 However, the single-layer PBI HFMs had very low tensile properties and were too fragile to fabricate modules. Kung et al. fabricated blended PBI/Matrimid single-layer asymmetric HFMs for toluene/iso-octane separation by pervaporation.158 The best performance was achieved with a flux of 1350 g m−2 h−1 and a separation factor of 200 using a toluene/iso-octane (50/50 wt%) mixture as the feed at a downstream pressure of 10 mbar.
To further improve the mechanical properties and separation performance of PBI HFMs, dual-layer PBI HFMs were made with the aid of co-extrusion spinning. P84 and PEI were chosen because they have excellent anti-swelling properties and good compatibility with PBI. The PBI/P84 dual-layer HFMs were fabricated for the dehydration of tetrafluoropropanol (TFP)141 and acetone142 using DCX cross-linked P84 as the porous substrate. Wang et al. used PEI as the inner support layer for ethylene glycol dehydration,106,149 and achieved far better performance than most other polymeric membranes with a separation factor up to 4524 and a flux of 186 g m−2 h−1. The PBI/PEI dual-layer HFMs were used for the dehydration of ethyl acetate and phenol. No delamination was observed at the interface between the two layers, indicating a good adhesion due to the miscibility of PBI and PEI.150,216 Comparing with single-layer PBI HFMs, dual-layer PBI HFMs showed higher mechanical strength and flexibility. The dual-layer co-extrusion technology could also reduce the PBI material cost and enhance the overall separation performance. Therefore, there is great prospect in developing PBI dual-layer HFMs for pervaporation separations by using other robust but low-cost materials as substrates. A performance summary of PBI HFMs for the dehydration of organic solvents and separation of solvent mixtures is listed in Table 5. Clearly, the inherently rigid structure, high hydrophilicity and good spinnability make PBI a promising membrane material for pervaporation applications.
PBI hollow fiber membrane | Feed composition (wt%) | T (°C) | Flux (g m−2 h−1) | Separation factor | Ref. |
---|---|---|---|---|---|
a DCX = p-xylene dichloride; P84 = BTDA-TDI/MDI co-polyimide; PEI = polyetherimide; TFP = tetrafluoropropanol. | |||||
m-PBI single-layer | Ethylene glycol/water (50/50) | 60 | 1147 | 116 (water/EG) | Wang et al. 2010 (ref. 106) |
m-PBI/P84 dual-layer | TFP/water (85/15) | 60 | 332 | 1990 (water/TFP) | Wang et al. 2007 (ref. 141) |
m-PBI/PEI dual layer thermally treated at 75 °C | Ethylene glycol/water (64/36) | 60 | 186 | 4524 (water/EG) | Wang et al. 2010 (ref. 106) |
m-PBI/PEI dual layer thermally treated at 75 °C | Ethylene glycol/water (80/20) | 60 | 115 | 1763 (water/EG) | Wang et al. 2011 (ref. 149) |
m-PBI/P84 dual-layer crosslinked by DCX and thermally treated at 250 °C | Acetone/water (85/15) | 50 | 300 | 490 (water/acetone) | Shi et al. 2012 (ref. 142) |
m-PBI single-layer crosslinked by DCX and thermal treated at 75 °C | Phenol/water (70/30) | 60 | 196 | 722 (water/phenol) | Wang et al. 2014 (ref. 150) |
m-PBI/PEI dual layer crosslinked by DCX | Ethyl acetate/water (98/2) | 60 | 820 | 2478 (water/ethyl acetate) | Wang et al. 2015 (ref. 216) |
m-PBI/Matrimid blend single-layer | Toluene/iso-octane (50/50) | 60 | 1350 | 200 (toluene/iso-octane) | Kung et al. 2010 (ref. 158) |
Since polymeric membranes are relatively inexpensive, resistant to sulfur compounds, and can be easily fabricated into large-scale, defect-free membranes and modules, they may be particularly suitable for H2 purification if the combustion turbines for power generation do not require high-purity H2.97 Unfortunately, most commercially available polymeric materials cannot withstand the high temperature of syngas exiting from the steam-reforming and water–gas shift reactions. The desirable polymeric membranes for syngas separation must be mechanically, chemically, and thermally stable at high temperature and pressures.
Since H2 has a smaller kinetic diameter than CO2 (2.89 vs. 3.3 Å), the former has higher diffusivity than the latter. To design a membrane with high H2/CO2 selectivity, one must choose the polymers and operation conditions that (1) increase the diffusivity selectivity (favoring the H2 permeate due to the size-sieving effect) and (2) suppress the solubility selectivity (favoring the condensable CO2) as the governing factors for the entire gas transport.73,168,227,228 In other words, the higher H2/CO2 selectivity arises from the combined effects: (1) H2 shows higher diffusivity increase with temperature than CO2 and (2) CO2 has lower solubility at higher temperatures. Owing to the relatively rigid polymer chains, small free volume fraction and high Tg, PBI is one of the unique materials that has the above characteristics for effective H2/CO2 separation.
Although PBI has an extremely low flux for H2 and CO2 at room temperature, its rigid structure and high Tg offer the needed diffusivity-based selectivity at temperatures above 150 °C.229 As the temperature increases, its H2 permeance increases faster than CO2 permeance, thereby increasing the H2/CO2 selectivity. The highly rigid PBI polymer chains also provide good resistance against CO2- and SO2-induced plasticization.230,231Table 6 summarizes the detailed H2/CO2 separation performance of recently developed PBI HFMs.81,82,109,132,167,168,232–237 Key achievements and major breakthroughs are highlighted as follows.
PBI hollow fiber membrane | Coating layer | Feed gas | ΔP | T (°C) | H2 permeance (GPU) | H2/CO2 selectivity (−) | Ref. |
---|---|---|---|---|---|---|---|
a 1 GPU = 1 × 10−6 cm3 (STP) cm−2 s−1 cmHg−1 = 7.50 × 10−12 m s−1 Pa−1. DBB = 1,4-dibromobutane; DBX = α,α′-dibromo-p-xylene; P84 = BTDA-TDI/MDI co-polyimide; PdNPs = palladium nanoparticles; sPPSU = sulfonated polyphenylsulfone; ZIF-8 = zeolitic-imidazole framework-8. | |||||||
PBI single layer | PBI-HFA | Pure | 5–8 x 106 Pa (5–8 bar) | 100 | 0.33 | 7.89 | Kumbharkar et al. 2011 (ref. 81) |
200 | 0.62 | 12.83 | |||||
300 | 0.99 | 21.74 | |||||
400 | 2.60 | 27.28 | |||||
tert-butyl PBI single layer cross-linked by DBB | Silicone rubber | Pure | 5–8 x 106 Pa (1–6 bar) | 20 | 12.97 | 3.16 | Kumbharkar & Li 2012 (ref. 232) |
m-PBI/zirconia/stainless steel composite membrane | — | Pure | 3.4 × 105 Pa (50 psia) | 250 | 4.67 | 43.0 | Berchtold et al. 2012 (ref. 233) |
Mixed syngas | 250 | 7.00 | 47.6 | ||||
m-PBI single layer | Defect-seal layer | Pure | N/A | 250 to 350 | 200–400 | >20 | Singh et al. 2014 (ref. 109) |
m-PBI single layer | — | Pure | 1.4 × 105 Pa (20 psia) | 250 | 9.72 | 17.11 | Dahe et al. 2019 (ref. 132) |
250 | 21.0 | 13.99 | |||||
250 | 7.56 | 22.37 | |||||
m-PBI/PdNP single layer | — | Pure | 1.0 × 105 Pa (1 bar) | 60 | 80 | 10 | Villalobos et al. 2018 (ref. 236) |
m-PBI single layer | 6F-PBI | Pure | 1.4 × 105 Pa (20 psia) | 95 to 350 | 90–400 | >20 | Singh et al. 2020 (ref. 82) |
m-PBI single layer | Silicone rubber | Pure | 7.0 × 105 Pa (7 bar) | 150 | 65 | 17.6 | Etxeberria-Benavides et al. 2020 (ref. 168) |
m-PBI/10 wt% ZIF-8 single layer | Silicone rubber | Pure | 7.0 × 105 Pa (7 bar) | 150 | 107 | 16.1 | Etxeberria-Benavides et al. 2020 (ref. 168) |
PBI-HFA single layer | — | Pure | 1.0 × 105 Pa (1 bar) | 24 | 10198 | 2.52 | Kim et al. 2021 (ref. 237) |
(m-PBI/10 wt% ZIF-8)/Matrimid® 5218 dual-layer HFM | — | H2/CO2 50:50 (v/v) | 7.0 × 105 Pa (7 bar) | 180 | 64.5 | 12.3 | Yang et al. 2012 (ref. 167) |
(m-PBI/33 wt% ZIF-8)/Matrimid® 5218 dual-layer HFM | — | H2/CO2 50:50 (v/v) | 7.0 × 105 Pa (7 bar) | 180 | 202 | 7.7 | Yang et al. 2012 (ref. 167) |
m-PBI:sPPSU (90:10)/polysulfone dual-layer HFM cross-linked by DBX and thermally treated at 120 °C | — | H2/CO2 50:50 (v/v) | 1.4 × 106 Pa (14 bar) | 90 | 16.7 | 9.7 | Naderi et al. 2019 (ref. 235) |
Coating m-PBI on P84 HFM support | Silicone rubber | H2/CO2 50:50 (v/v) | 6.0 × 105 Pa (6 bar) | 180 | 39 | 20.2 | Sánchez-Laínez et al. 2021 (ref. 234) |
Kumbharkar et al. fabricated m-PBI HFMs using DMAc/water as a bore fluid and water as an external coagulant and then coated them with 6F–PBI to seal the defects for H2/CO2 separation at 100–400 °C.81 It was found that the bore fluid chemistry played an important role in determining membrane morphology, gas separation performance and mechanical strength. The resultant HFMs had a H2 permeability of 2.6 GPU and a H2/CO2 selectivity of about 27 at 400 °C. Kumbharkar and Li also synthesized tert-butyl-PBI and fabricated it as asymmetric PBI HFMs using a dry-jet wet spinning approach.232 The HFMs were crosslinked by 1,4-dibromobutane (DBB) and then dip coated with silicone rubber to seal the surface defects. Fig. 18 illustrates the crosslinking scheme between tert-butyl-PBI and DBB. The tert-butyl group substitution disrupted the PBI molecular chains and increased the FFV. Thus, the modified-PBI HFM membranes exhibited good separation performance for gas pairs such as CO2/N2, O2/N2 and H2/N2. For H2/CO2 separation, they had a higher H2 permeance of 12.97 GPU but a lower H2/CO2 selectivity of 3.16 at 20 °C.
Fig. 18 The mechanism of crosslinking reaction between tert-butyl-PBI and DBB.232 |
Berchtold et al. fabricated a PBI-stainless steel composite membrane by depositing a thin m-PBI layer through a proprietary process on the outer surface of a porous stainless-steel support consisting of an intermediate zirconia layer.233 The PBI membrane module was tested for H2/CO2 separation from 150 to 250 °C in simulated dry syngas. It had a H2 permeance and H2/CO2 selectivity of 7 GPU and 47 respectively at 250 °C, surpassing the 2008 Robeson's upper bound for H2/CO2 separation. Moreover, even in the presence of H2S, the PBI composite membrane showed long-term stability without any performance degradation.
As mentioned in Section 3.2, both Dahe et al.132 and Singh et al.82 investigated the effect of coagulant chemistry on the removal of macrovoids from PBI HFM morphology. Today, the technologies to develop PBI HFMs with a highly interconnected and thermo-mechanically porous sub-layer have been established for H2/CO2 separations. Fig. 19 shows their typical morphology. After being annealed at 375 °C and coated with a 6F-PBI sealing layer, the resultant PBI HFMs showed commercially competitive permselectivity characteristics. They had a H2 permeance of 200–400 GPU and a high ideal H2/CO2 selectivity of >20 at 250 to 350 °C.
Fig. 19 Typical morphology of polybenzimidazole hollow fiber membranes for gas separation. Reproduced with permission from ref. 109, copyright 2014, Elsevier. |
In terms of PBI composite HFMs, Sánchez-Laínez prepared composite PBI/P84 HFMs by coating a thin PBI selective layer on a P84 HFM support using an m-PBI solution containing NaOH and ethanol.234 After the silicone rubber coating, the PBI/P84 hollow fibers showed a H2 permeance over 39 GPU with a H2/CO2 selectivity of 20.2 using a mixed H2/CO2 gas of 50:50 v/v as the feed at 7 bar and 180 °C. Naderi et al. fabricated dual-layer HFMs consisting of an outer-selective layer made of a PBI and sPPSU blend and a polysulfone inner-layer substrate.235 sPPSU was chosen as an ionic-crosslinker so that the DBX modified PBI had a higher permeability than the pristine PBI. The resultant HFMs had a H2 permeance of 16.7 GPU and an H2/CO2 selectivity of 9.7 at 90 °C and 14 bar.
PBI HFMs spun from MMMs were also developed using ZIFs as nanofillers. Yang et al. fabricated PBI/Matrimid dual-layer HFMs by incorporating ZIF-8 nanoparticles in the PBI selective layer.167 The dual-layer HFMs were defect-free, without post-annealing and coating, but by optimizing ZIF-8 nanoparticle loadings, spinning conditions, and solvent-exchange procedures. When being tested at 180 °C using a H2/CO2 gas mixture (50:50 v/v) as the feed at 7 bar, two types of PBI HFMs were developed for hydrogen purification at high temperatures: (1) the HFMs containing 10 wt% ZIF-8 had a medium H2 permeance of 64.5 GPU and a high selectivity of 12.3 and (2) the HFMs containing 33 wt% ZIF-8 had a high H2 permeance of 202 GPU and a medium selectivity of 7.7. Moreover, the presence of CO and water vapor in the feed stream had no significant effects on membrane performance. Etxeberria-Benavides et al. fabricated defect-free PBI/ZIF-8 MMM HFMs comprising a thin dense layer of 300 nm by dispersing 10 wt% ZIF-8 into the PBI polymer matrix.168 Comparing with pure PBI HFMs, the PBI MMM HFMs showed great increase in H2 permeance from 65 GPU to 107 GPU at 150 °C and 7 bar, while the ideal H2/CO2 selectivity remained constant at 16.1. However, they found that the incorporation of ZIF-8 into the PBI polymer matrix could strongly influence gas transport, specifically in mixed gas tests. The enhanced H2/CO2 separation was compromised at high pressures of 30 bar owing to the strong CO2 adsorption in the nanocavities of ZIF-8 that would suppress the H2 transport.
With the aid of palladium nanoparticles (PdNPs), Villalobos et al. fabricated defect-free PBI/PdNP HFMs consisting of a thin dense skin layer filled with PdNPs by combining the complexation induced phase separation (CIPS) and NIPS processes,236 as shown in Fig. 20. Palladium was added into the membrane in the form of ions to coordinate with the imidazole groups of PBI and minimize its agglomeration. The PBI/PdNP composite HFMs not only showed higher permeance than the pristine PBI membranes but also maintained the stability of Pd nanoparticles due to the synergistic effects between PdNPs and the PBI matrix. The resultant PBI/PdNP HFMs made from a Pd(OAc)2 concentration of 50 × 10−5 mol L−1 had a H2 permeance and H2/CO2 selectivity of 80 GPU and 10 at 60 °C, respectively. As shown in Fig. 21, the performance of PBI hollow fiber membranes for H2/CO2 separation has gradually surpassed the upper bound of 2008 Robeson's curves.65,238
Fig. 20 Spinning process developed to make hollow fibers with a palladium-rich selective dense layer. (a) Diagram of the triple-orifice spinneret showing the orifice used for each solution and the two precipitation processes that take place (i.e., CIPS and NIPS); (b) photograph of the PBI/PdNP hollow fiber before (left) and after (right) the reduction step to convert the Pd ions to PdNPs. Reproduced with permission from ref. 236, copyright 2018, John Wiley & Sons. Permission conveyed through Copyright Clearance Center, Inc. |
Fig. 21 Robeson's plot comparing the PBI hollow fiber membranes for H2/CO2 separation. The line represents the 2008 Robeson's upper bound.65,238 |
Other efforts have been made to (1) blend PBI with thermosets in order to improve the thermal stability,239 (2) embed soluble organic macrocyclic cavitands (sulfocalixarenes, SCA) to form homogeneous PBI nanocomposite membranes with distinctly molecular-sieving nanocavities,164,240 (3) grow a selective MOF layer on the PBI HFM surface,241 (4) dope PBI membranes with a polyprotic acid to improve H2/CO2 diffusivity selectivity,40 (5) apply Pd alloy (PdAg and PdNi) nanowires in PBI mixed matrix membranes to increase hydrogen diffusivity and reduce Pd embrittlement and susceptibility to poisoning,242 (6) control the degree of N-quaternization on PBI based polymeric ionic liquids (PILs) to improve CO2 sorption and gas permeation,243 and (7) carbonize PBI as a carbon molecular sieve (CMS) with greatly enhanced H2/CO2, O2/N2 size-sieving ability.244,245 These schemes may potentially enhance the separation performance of PBI-based HFMs if one can successfully and economically convert them from flat-sheet configurations to hollow fibers. Future studies should also be focused on their scalability, long-term performance, and techno-economic analyses for H2/CO2 separation at high temperatures.
• Although advances in the fundamentals of single-layer hollow fiber formation and the state-of-the-art macrovoid-free PBI HFMs with an ultrathin dense-selective layer have been established, they are only applicable for the use of m-PBI (i.e., commercially available Celazole® PBI). Since the optimal composition of the PBI-based dense-selective layer is still under extensive studies, it could be still a challenging task to design a defect-free integrally skinned asymmetric PBI HFM consisting of a tailored morphology and a tuneable dense-selective layer spun from MMMs or nanocomposite materials.
• The dual-layer co-extrusion technology should receive more attention in future R&D because it has the advantages of significantly reducing material costs and substructure resistance as well as enhancing the membrane's mechanical strength if a low-cost but robust material is employed as the support layer. So far, dual-layer PBI HFMs have demonstrated superior performance to single-layer ones in OSN and pervaporation as well as common gas separations at ambient temperature. Their applicability to H2/CO2 separation at high temperatures is a challenging task for further studies.
• The scalability, long-term performance, and techno-economic analyses of the aforementioned PBI HFMs must be conducted for actual industrial applications. This is especially imperative for H2/CO2 separation because (1) the methane steam reforming process produces syngas comprising multiple complicated components at high temperatures, and (2) the newly developed H2-selective PBI-based HFMs have to survive in these harsh environments for a long period of operation time.
• To facilitate the commercialization of H2-selective PBI-based HFMs for high-temperature applications, the highly permeable material 6F–PBI or PBI–HFA must be commercially available. Thus, similar to the use of silicone rubber materials to seal defects of conventional HFMs for O2/N2 and CO4/CH4 separations, a facile and cost-effective sealing procedure can be adopted for each PBI-based HFM for hydrogen recovery at high temperatures.
Molecular modelling and simulation have played an important role in advancing the fundamental understanding of membrane formation, material design and selection, and various separation mechanisms across membranes.246–249 So far, the architecture designs of PBIs, PBI/nanocomposite materials and MMMs, and their membrane formation have not been exclusively examined at a molecular level. It is envisioned that the combination of material simulation and advanced experiments may help build the relationships among polymer formulation, processing parameters, structural and mechanical analyses and separation performance that facilitate the development of next generation PBI-based membranes with precise separation. Given the unique and superior properties of PBI membranes, new demands for other separation methods may emerge for applications in the chemical, petrochemical, food, and pharmaceutical industries.
2-MeTHF | 2-Methyl tetrahydrofuran |
AEM | Anion exchange membrane |
API | Active pharmaceutical ingredients |
BDA | Butanediamine |
BILP | Benzimidazole-linked polymer |
CA | Cellulose acetate |
CIPS | Complexation induced phase separation |
CMS | Carbon molecular sieve |
CO2 | Carbon dioxide |
DAB | 3,3′-Diaminobenzidine |
DBB | 1,4-Dibromobutane |
DBX | α,α′-Dibromo-p-xylene |
DCM | Dichloromethane |
DCX | α,α′-Dichloro-p-xylene |
DEO | 1,2,7,8-Diepoxyoctane |
DMAc | Dimethylacetamide |
DMF | Dimethylformamide |
DMSO | Dimethyl sulfoxide |
ED | Electrodialysis |
EG | Ethylene glycol |
FFV | Fractional free volume |
FO | Forward osmosis |
GA | Glutaraldehyde |
GO | Graphene oxide |
HFA | 4,4′-(Hexafluroisopropylidene)bis(benzoic acid) |
HFM | Hollow fiber membrane |
HPEI | Hyperbranched polyethyleneimine |
IPN | Interpenetrating polymer network |
ISA | Integrally skinned asymmetric |
MBRs | Membrane bioreactors |
MCDI | Membrane capacitive deionization |
MeCN | Acetonitrile |
MF | Microfiltration |
MMM | Mixed matrix membrane |
MOF | Metal–organic frameworks |
MPC | Metal–polymer coordination |
MW | Molecular weight |
MWCO | Molecular weight cut off |
NASA | National Aeronautics and Space Administration |
NF | Nanofiltration |
NIPS | Non-solvent induced phase inversion or separation |
NMP | N-Methyl-2-pyrrolidone |
NS | Non-solvent |
OSN | Organic solvent nanofiltration |
P84 | Co-polyimide, BTDA-TDI/MDI |
PAN | Polyacrylonitrile |
PBI | Polybenzimidazole |
PBI-OH | Hydroxylated polybenzimidazole |
PDA | Polydopamine |
PdNPs | Palladium nanoparticles |
PEI | Polyetherimide |
PEM | Polymer electrolyte membranes |
PES | Polyethersulfone |
PI | Polyimide |
PILs | Polymeric ionic liquids |
PIM | Polymer of intrinsic microporosity |
POF | Porous organic framework |
POSS | Polyhedral oligomeric silsesquioxane |
PPA | Polyphosphoric acid |
PPL | Polypyrrolone |
PPMA | Phosphorus pentoxide/methanesulfonic acid |
PPSU | Polyphenylsulfone |
PRO | Pressure-retarded osmosis process |
PSA | Pressure swing adsorption |
RO | Reverse osmosis |
SG | Sulfonated graphene |
sPPSU | Sulfonated polyphenylsulfone |
TAPDS | Tetraaminodiphenylsulfone |
TBB | 1,3,5-Tris(bromomethyl)benzene |
TCL | Terephthaloyl chloride |
TDI | Toluene 2,4-diisocyanate |
TFC | Thin film composite |
TFP | Tetrafluoropropanol |
TG | Glass transition temperature |
TGIC | Triglycidylisocyanurate |
THF | Tetrahydrofuran |
TMC | Trimesoyl chloride |
UF | Ultrafiltration |
XDA | p-Xylenediamine |
ZIF | Zeolitic imidazolate frameworks |
δ T | Total solubility parameter of a material |
δ d | Solubility parameter contributed by dispersion forces |
δ p | Solubility parameter contributed by polar interactions |
δ h | Solubility parameter contributed by hydrogen bonding |
This journal is © The Royal Society of Chemistry 2022 |