Dipti. R.
Sahu
*a,
Cheng-Yen
Hung
b,
Sheng-Chang
Wang
c and
Jow-Lay
Huang
bde
aDepartment of Natural and Applied Sciences, Namibia University of Science and Technology, Private Bag 13388, Windhoek, Namibia. E-mail: dsahu@nust.na; Fax: +264-6-2079783; Tel: +264-6-2072783
bDepartment of Materials Science and Engineering, National Cheng-Kung University, Tainan, 701, Taiwan
cDepartment of Mechanical Engineering, Southern Taiwan University of Science and Technology, Tainan, 710, Taiwan
dCenter for Micro/Nano Science and Technology, National Cheng Kung University, Tainan, 701, Taiwan
eHierarchical Green-Energy Materials (Hi-GEM) Research Center, National Cheng Kung University, Tainan, 701, Taiwan
First published on 13th June 2022
Nanostructured electrochromic materials having long life cycle and high chemical stability are promising for displays, rear view mirrors, and smart window applications. In the present study, nano tungsten trioxide (WO3) films are prepared using a low-cost conventional spin coating method. The porosity of the WO3 layers is developed using a polystyrene intermediate layer in order to improve the cyclic stability of the film. The structural characterization using X-ray diffraction confirms the formation of the orthorhombic phase. Surface studies via atomic force microscopy and scanning electron microscopy show a porous network along with a change in the roughness of the films. Electrochromic study using a potentiostat, UV-visible spectrophotometer and the voltammetry method indicate that a porous crystalline WO3 has a stable coloration efficiency, durability, and fast response to the electrochromic cycle with higher transmittance in comparison with nonporous WO3 films. The crystalline film with a porous structure shows a transmission modulation of about 65.3% and 10% more coloration efficiency than the nonporous film. The electrochromic properties of the crystalline nonporous film deteriorate at/after 500 °C. The porous structure improves the chemical stability of the film with long durability and solves the problem of degradation of the film after long hours of operation for an electrochromic device.
Since the first reported work on the electrochromism of WO3,7 this material has been continuously researched for improving its properties, understanding its physics and developing devices using WO3.6,8–10 In general, there are interstitial sites in WO3 where foreign materials or ions can be inserted easily to change the behaviour of the EC material.11,12 It is known that in its fully occupied state WO3 is transparent but it reaches the EC state after electrochemical reduction.13
Currently, the anodic oxidation method is normally used for the manufacture of WO3 thin films.14,15 Porosity, thickness, crystallinity, composition, and stoichiometry are important factors that influence the electrochromic properties of WO3 thin filmw.16–19 Our previous study on a WO3 film synthesized by a chemical method shows that the film exhibited optimum electrochromic properties in its crystalline phase; however, the chemical stability and coloration efficiency of the film deteriorates after a long cycle of operation.20 Therefore, there is a need to improve the electrochromic behaviour of the film by maintaining the stability of the electrochromic properties during applications. It is reported that a high film porosity will enhance the surface area and improve the electrochromic properties of films.21,22 The growth of a porous electrochromic film can increase the color/bleach rate, extend durability, stabilize electrochromic properties, and increase its lifetime.1,6,12 The production of environment friendly WO3 can advance the research in the electrochromic film fabrication and its application in glass window films. The goal of this study is to improve the chemical stability of the film by prolonging the cyclic durability and improving the electrochromic properties without degradation for device application. Therefore, in this study, nano porous WO3 films are prepared with a solgel processed precursor solution using a low-cost conventional spin coating method. The porosity of the WO3 layers is generated using the polystyrene as an intermediate layer. The porous crystalline WO3 film shows a stable coloration efficiency of 24 cm2 C−1, transmittance modulation effect of 65.3% and good electrochromic properties up to 1000th cycle of operation, which is much better than other reported literature data.20–23 In literature, only few doped films show good coloration efficiency but they degrade after long cycle of operations, while other few films are not stable without doping that changes the electrochromic properties after a cycle of operation.22,23 Herein, the observed electrochromic properties are much better in the prepared pure porous crystalline WO3 film in terms of coloration efficiency and transmission modulation compared with nonporous WO3 films.
The structural properties of the prepared films were studied by a D/Max-II X-ray diffractometer (XRD) with CuKα radiation. The surface morphology the films was studied using a XL 40 Philips scanning electron microscope (SEM) at an operative voltage of 10 kV. The accelerating voltage of the SEM was in the range of 5–30 kV. Atomic force microscopy (AFM) images were acquired using a Digital Instrument INC, NanoScope, California, USA. The electrochromic properties of the films were studied by cyclic voltammetry. The cyclic voltammogram test was carried out on a Versastat II electrochemical workstation of a three-electrode cell system with an electrolyte solution of 0.5 M lithium perchlorate in propylene carbonate (LiClO4/PC). The working electrode was made of tungsten oxide film on the ITO substrate. The reference and counter electrodes were a saturated calomel electrode (SCE) and a platinum grid, respectively. The transmittance spectra of the films were recorded in the 300–800 nm wavelength range using the Hitachi U-2001 UV-visible spectrophotometer.
Fig. 1 presents the SEM micrograph of the WO3 film. The surface morphology of the film shown in Fig. 1(a) indicates that the polystyrene latex microsphere dispersed in 2.5 wt% water is well deposited on the surface of the WO3 layer. The polystyrene latex microsphere ranges between 185 nm and 215 nm in size. The film with a single layer of WO3 deposited with the polystyrene sphere looks smooth and well arranged. Fig. 1(b) presents the porous structure on the annealed film at 300 °C where another layer of WO3 is deposited on the polystyrene sphere. The WO3 film looks porous with a nanoscale interconnecting network, which is similar to the reported literature.27 The WO3 film looks like a random porous island structure. Fig. 1(c) shows the micrograph of the crystalline WO3 film annealed at 500 °C. The morphologies of the WO3 film show changes in the structure. The WO3 pore sizes increase with the annealing and change the film behaviour as the film becomes fully crystalline. The porous WO3 film may have more open space among the materials, which allows the polystyrene sphere to penetrate through the film and make the film well defined by the crystalline structure. This nanoporous morphology and structure with the intragranular contact effectively improve the electrochromic behaviour of the film, which can be controlled by the polystyrene sphere and annealing temperature.28,29
Fig. 1 SEM micrograph of the WO3 film (a) polystyrene latex microsphere (b) annealed porous film (c) porous crystalline film. |
Fig. 2(a and b) shows the atomic force micrograph of the crystalline and porous crystalline WO3 films, respectively. The images show a roughness value of about 2.08 nm (Fig. 2(a)) for the nonporous crystalline film, which increases to 69.02 nm (Fig. 2(b)) for the porous crystalline film. However, the roughness of the as deposited film is 13.92 nm (images not shown here) that decreases to 2.08 nm by annealing at 500 °C temperature. This indicates that the polystyrene sphere, which is porous in structure, can change the roughness of the film with annealing. The annealed porous crystalline films are much rougher than the as-deposited amorphous films.30
Fig. 2 AFM images of the as-deposited and annealed (a) crystalline and (b) porous crystalline WO3 films. |
The potential step spectrum of the WO3 films present in Fig. 3 for the nonporous and porous crystalline states indicates that the porous crystalline WO3 films have an insertion ability of about 39.9 mC, which is higher than the nonporous crystalline film. This indicates that when the film becomes porous, an increase in the surface area is observed, and thus, the ion insertion capability increases apparently, which enhances the electrochromic behaviour of the film.31
Fig. 4 presents the transmittance spectra of nonporous and porous crystalline WO3 films. The transmittance spectra for the nonporous film are more porous than the crystalline film in colored state. There is no significant difference between the transmittance spectra. However, the trend of transmittance spectra is different for both films. For the nonporous crystalline film, the transmittance is increasing in the visible region and then it decreases in the long wavelength region. On the contrary, the porous crystalline film trend initially decreases in the visible region, and then it increases continuously in the long wavelength region up to 1100 nm. The maximal transmittance of the porous film increases to 25% while the nonporous film is reduced to 10%. In the visible region, the maximum transmittance of about 60% is achievable for the crystalline nonporous film. However, in the bleached state, both films show higher transmittances. The porous crystalline WO3 film exhibits a transmittance modulation effect of 65.3%. However the nonporous film shows a modulation of 34.6%. The nonporous film shows more than 30% modulation in the colored and bleached states. Due to the increase in the surface area in the porous film, more charge intercalation occurs, which affects the transmittance of the films. The detailed electrochromic results are listed in Table 1.
Fig. 4 The transmittance spectra of nonporous and porous crystalline WO3 films in coloured and bleached states. |
Crystalline without porous | Crystalline with porous | |
---|---|---|
ΔT (%) | 34.6 | 65.3 |
Q in (mC) | 24.12 | 39.9 |
CE (cm2 C−1) | 14.12 | 24 |
Fig. 5 shows the electrochromic cyclic voltammogram (CV) curves for the porous crystalline films at different cycles of operation. The CV curves indicate that there is a change in the peak positions with the incorporation of an injected charge.32 The film shows good electrochromic behaviour up to the 1000th cycle of operation and there is a decrease in the integral area during the operation cycle. This indicates that the electrochemical reaction is occurring in the film during the cycle of operation. The films show stable electrochromic properties. The porous crystalline film is not degraded after the operation.
Fig. 5 The electrochromic cyclic voltammogram (CV) curves for the porous crystalline films for different cycles of operation. |
The durability of the films after the electrochromic cycle is studied in terms of charge intercalation, and the results are shown in Fig. 6. It is observed that there is a variation in charge intercalation for each film after the cycle of operation. The charge intercalation increases for the crystalline film, almost remains constant for the porous crystalline film, and decreases rapidly for the amorphous films. The effect of grain boundary and reaction generally changes the relative capacity of charge intercalation in the film. The porous crystalline film shows a good crystalline structure and uniform grain size; therefore, it maintains almost the same amount of charge intercalation after a long cycle of operation. The film structure, morphology and electrolytes affect the intercalation/deintercalation processes.33,34 This charge intercalation also affects the transmittance modulation and cyclic life of the film.35 In this study, the porous film shows stable and improved electrochromic properties as porous crystalline film aggregation does not take place and the film did not reach its steady state.
Fig. 6 Q in/Qmaxvs. cycle's spectrum of WO3 films at amorphous, porous crystalline and crystalline states. |
The coloration efficiency (CE) defined as CE = ΔOD/Qin,36 where ΔOD is the change in the optical density with charges intercalated per unit electrode area and Qin is the charge intercalated per unit area, is used to study the intrinsic material property. Herein, ΔOD = log (Tbleaching/Tcoloring) where Tbleaching is the transmittance in the bleached state and Tcoloring is the transmittance in the colored state. The CE analysis shows that the porous crystalline film has 24 cm2 C−1 efficiency while the crystalline film has 14 cm2 C−1. The CE is almost constant up to the 1000th cycle for the porous crystalline film mainly due to the constant amount of charge intercalation during the long cycle of operation.37,38 This indicates that the grown film has good durability. However, the CE is not constant for the amorphous film during the cycle of operation. This may be due to the change in the charge intercalation during the cycle of operation.39,40 As there is no change in the CE value after the long cycle of operation, it indicates that the films are of good quality with stable morphology after the electrochromic cycle.41–43 In our earlier study,20 it was found that the electrochromic coloration behaviours of the amorphous and crystalline films are not stable, the transmission modulation decreases, and films degrade after long cycles of operation. However, this porous crystalline film shows stable coloration efficiency, durability, and fast response to the electrochromic cycle with higher transmittance, which are prerequisites for smart window applications. The growth of the porous electrochromic film can solve the problem of the degradation of the film after long hours of operation in a device.
This journal is © The Royal Society of Chemistry 2022 |