This review outlines the design strategies which aim to develop high performing n-type materials in the fields of organic thin film transistors (OTFT), organic electrochemical transistors (OECT) and organic thermoelectrics (OTE). Figures of merit for each application and the limitations in obtaining these are set out, and the challenges with achieving consistent and comparable measurements are addressed. We present a thorough discussion of the limitations of n-type materials, particularly their ambient operational instability, and suggest synthetic methods to overcome these. This instability originates from the oxidation of the negative polaron of the organic semiconductor (OSC) by water and oxygen, the potentials of which commonly fall within the electrochemical window of n-type OSCs, and consequently require a LUMO level deeper than ∼−4 eV for a material with ambient stability. Recent high performing n-type materials are detailed for each application and their design principles are discussed to explain how synthetic modifications can enhance performance. This can be achieved through a number of strategies, including utilising an electron deficient acceptor–acceptor backbone repeat unit motif, introducing electron-withdrawing groups or heteroatoms, rigidification and planarisation of the polymer backbone and through increasing the conjugation length. By studying the fundamental synthetic design principles which have been employed to date, this review highlights a path to the development of promising polymers for n-type OSC applications in the future.
Herein, this review will focus on electron transporting OSC polymers, and the considerations necessary for designing materials suited to the desired application. The prototypical n-type device for OSCs is the organic thin film transistor (OTFT), so the rationale behind the design of OSCs for n-type OTFTs is first discussed. A clear understanding of the features and properties of these structural motifs enables analysis of their further adaptation for application in the emerging n-type OSC based technologies, namely organic electrochemical transistors (OECT) and organic thermoelectric (OTE) generators. Current literature on polymeric OSCs is dominated by the high performance of p-type materials, whilst the development of electron transporting materials has consistently lagged. Improvements in n-type materials for OTFTs and OECTs are necessary to allow for the creation of complementary logic circuits, built with well-matched p-type materials, which lower the static power consumption, enabling faster circuit speeds, more complex circuits and increased operational stability.7–9 OTE generators also require OSCs for both p-type and n-type operation with well-matched electrical and thermal conductivities. To discuss the design of materials, first we must address the relationship between conjugation, charge transport and morphology, alongside the fundamental challenges with n-type materials and why high performing n-type materials are relatively scarce.10 It should be noted that theoretically the transport mechanisms utilised by electrons and holes are identical, so are not the limiting factor in the inferior performance of n-type materials.11
The efficiency of charge transport in polymeric OSCs is governed by a number of factors both intrinsic to the polymer and dependent on device properties. Factors relating to the chemical structure of the polymer include reorganisation energy and transfer integrals, which in turn are influenced by the frontier molecular orbital energies and distributions, as well as the polymer conformation, molecular weight and sidechain composition.12–15 Device dependant factors include thin film morphology, charge carrier density, charge injection barriers and charge trapping.16–18 For example, the molecular weight of polymeric OSC materials can have a significant impact on the mobility of a material.19 This can be explained by noting that longer polymer chains act as connectors between crystalline regions within the microstructure (Fig. 1(a)). Without these, clear paths between ordered domains are limited and mobility is greatly reduced. It has been proposed, however, that for electron transporting polymers utilising a naphthalenediimide (NDI) backbone, the molecular weight is a less important factor for two reasons, the first being that the NDI unit can undergo a two-fold reduction to the dianion, thus charge remains localised on the NDI unit.20 The second reason is the degree of aggregation observed in solution, which reduces for lower molecular weight samples, resulting in more ordered backbones and larger regions of crystallinity.21 This second point also poses the question of the best methods for establishing the molecular weight of polymers, particularly where a material exhibits significant aggregation in solution. In these cases, the common method of using size exclusion chromatography, which includes gel permeation chromatography (GPC), may not be sufficient, and alternative methods, such as end group NMR spectroscopy analysis, to identify the absolute number of protons and determine the molecular weight may be required.22
Fig. 1 Graphic representation of the microstructure of a variety of polymeric materials. (a) Semi-crystalline polymer, (b) partial order due to short-range aggregates and (c) an amorphous structure. The yellow shading indicates ordered regions, and long polymer chains, indicated in yellow, represent clear “paths” for charge transport, significantly improving charge transport. Figure adapted from literature.23 |
A higher mobility is often recorded when defects and impurities in the material are minimised, thereby reducing the number of trapping sites and subsequently decreasing the number of immobile charge carriers. OSC polymers are most commonly semi-crystalline, with regions of crystallinity, dispersed in amorphous regions (Fig. 1). These regions of crystallinity can be categorised more specifically into areas of long- and short-range order.23 Charge transport occurs throughout the highly ordered regions as far as possible to avoid the large energy barrier associated with charges moving from ordered to amorphous regions. Unfortunately, transport through disordered domains is unavoidable and is often the bottleneck for charge transport in OSC polymers. Where charge transport must occur through amorphous regions, it is possible to assist this by ensuring polymer chains are of sufficient length to act as tie chains between regions of crystallinity.24–26
As such, materials that efficiently transport charge and are deemed “high mobility” generally contain adequate regions of high order, with short connecting sections of amorphous material.27 An example of a high-mobility n-type polymer is the branched NDI derivate P(NDI2OD-T2), where large regions of crystallinity have been observed.28 This polymer also takes advantage of a face-on packing texture,29 with the aromatic polymer backbones stacked directly on top of each other, parallel to the substrate. This facilitates the hopping mechanism of electrons between chains, due to a stronger orbital overlap and interchain interaction.
In summary, more efficient packing leads to improved charge carrier transport, higher mobilities29 and short contact distances.30–33 Factors which alter the packing of a material are strong dipole–dipole interactions,34,35 degree of backbone planarity and steric locking of polymer backbones.36,37
Fig. 2 (a) The key reduction equations that cause inherent n-type thermodynamic instability and their associated energies. The redox potentials are measured versus the standard calomel electrode (SCE) at pH = 7.47 The corresponding LUMO levels have then been approximated from these redox potentials using the equation ELUMO = Ered + 4.4 V.47 pol− represents the anionic polymer species undergoing the redox reaction, which has an associated overpotential. (b) A schematic representation of the stability requirement of the LUMO energy level of an n-type material. This takes into account an overpotential of 0.9–1.0 eV, which is associated with the energetic barriers originating from penetration of the ambient species into the semiconducting material.50 Stability can generally be improved via two methods: either by operating devices under inert conditions or by designing materials with deeper LUMO levels. |
More specifically, water is reduced at potentials lower than −0.658 V (−3.7 eV), and oxygen can undergo reduction to hydrogen peroxide by electron transfer from the excited OSC negative polaron to a dioxygen molecule at +0.024 V (−4.4 eV).47,48 Oxygen can also undergo a four electron reduction at +0.571 V (−4.9 eV), so without taking overpotentials into account, for an n-type polymer to be stable to water, the doped (reduced) polymer should be oxidised at a potential higher than −0.658 V, furthermore for it to be stable to both oxygen and water, it needs to be oxidised higher than +0.571 V (Fig. 2).47 This initially appears unachievable, however, it has been empirically observed that a LUMO level below ∼−4 eV is necessary to ensure stability in ambient conditions.49 This can be explained through the concept of overpotentials, which is a free energy of activation that is required for the reaction to proceed, thus an excess voltage compared to the theoretically derived number is required to provide this free energy.47 In other words, although the reduction is thermodynamically favourable, it is kinetically hindered. This has been exemplified in studies investigating the stability of OTFTs based on OSCs with progressively deeper LUMO levels, from which an overpotential of around 0.9–1.0 eV was determined, which corresponds to a LUMO of −4 eV.49 The magnitude of the excess voltage will also be dependent on the OSC and the device configuration in which it is employed. Bearing this in mind as a design strategy moving forward is crucial if any attempts are to be made at creating thermodynamically stable n-type OSCs.
Oxygen can also be a threat to the stability of an OSC through the generation of singlet oxygen (1O2), which is formed by an energy transfer from the excited OSC triplet state, arising from intersystem crossing from the excited singlet state, to the triplet ground state of oxygen (3O2). This 1O2 is then able to undergo a 1,4 Diels–Alder addition in thiophene containing polymers, which leads to photobleaching.48 The simple solution to this is to encapsulate the device, removing all light sources, however this type of degradation must be predicted and accounted for in order to prevent it. OSC stability can also be improved by considering the close packed distances between polymer chains. Minimising these, for example through crystallisation, can provide a kinetic barrier to the diffusion of oxygen into the film, thus improving operational stability.8,36,51
Aside from the stability issues, a generic explanation for poor performance of n-types can be understood by examining the delocalisation of the LUMO in n-type polymers compared to that of the highest occupied molecular orbital (HOMO) in p-type polymers. In high performing p-type OSCs, while the HOMO may be slightly more prominent on the electron rich moiety, the HOMO is generally delocalised across the polymer backbone.52,53 This is not the case in common n-type materials, where the LUMO is more typically highly localised on the electron deficient component, causing electrons to become confined to the acceptor motif and electron mobility to decrease.40
Trapping of electrons in n-type OSCs can also occur on account of the device architecture, for example when employing silicon oxide substrates for n-type OTFTs, it has been shown that passivating the pendant hydroxyl groups by using a buffer dielectric/surface passivation is particularly important to prevent charge trapping, especially for n-type materials with shallow LUMO levels.4,40
Herein, we will discuss some fundamental properties and generic underlying design principles for electron transporting OSC materials, including synthetic manipulations of the energetics and optoelectronics of these materials, as well as providing high performing examples from literature.
Fig. 3 (a) Schematic of a donor–acceptor copolymer, (b) hybridisation of the molecular orbitals of the donor and acceptors monomers of a generic copolymer, and (c) an example of a donor–acceptor copolymer, N,N′-dialkylnaphthalenedicarboximide-dithiophene (NDI2OD-T2).28 |
One of the main synthetic reasons for D–A copolymers being so readily available for organic device applications is due to transition metal mediated coupling steps, which are facilitated by one of the two monomers having an electron rich conjugated system. The first high performing n-type material, poly{[N,N′-bis(2-octyldodecyl)-naphthalene-1,4,5,8-bis(dicarboximide)-2,6-diyl]-alt-5,5′-(2,2′-bithiophene)} (NDI2OD-T2), also known as N2200 (Fig. 3(c)), has such a D–A motif.28 This copolymer exhibits a relatively deep LUMO (approximated through a large EA value of 3.9 eV), facilitating electron injection and giving reasonable stability.28 More generally, n-type materials tend to comprise of a selection of electron deficient units, including naphthalenediimide (NDI),55 diketopyrrolopyrrole (DPP)56 or isoindigo (IIG).57
The synthetic techniques for deepening the LUMO level of an OSC include extending the conjugation length,58,59 the introduction of heteroatoms into the polymer backbone,60–62 decreasing the dilution effect to reduce the electron density in the polymer backbone,63 increasing backbone planarization,36,64,65 addition of electron-withdrawing groups,62,66,67 and the use of an all acceptor motif to delocalise the LUMO (Fig. 4).36,68 These design strategies are explored in more detail in further material examples in the forthcoming sections.
Fig. 4 A summary of design strategies to deepen the LUMO level, which in turn improves n-type stability and performance. |
Nitro, carboxyl, cyano and fluorine functionalities are examples of electron-withdrawing substituents through both inductive and resonance effects. These groups can also be combined with the use of alternating donor and acceptor monomers, to further reduce the electron density of the accepting component (Fig. 4).54 Alkyl sidechains are not only beneficial for promoting solubility of otherwise insoluble aromatic cores, but additionally have been shown to influence the molecular packing and charge transport properties of a material.69 This can either be beneficial or detrimental depending on the sidechain selection and their interaction, for example where a material exhibits interdigitation (e.g. as expected with PTEG-170), long range order is achieved, and therefore mobility is increased.71,72 However, where branched chains are required to impart sufficient solubility, they can significantly impede charge transport.73 One solution is the introduction of a linear spacer between the backbone and the branching point, which maintains good close-contact distances and allows for solution-processability of the material.74–76 Other solubilising sidechains have also been explored in the field of OSCs,77 including those with ionic functionalities,78 hydrosilanes79 and most notably oligo(ethylene glycol) (OEG) chains,80–82 which will be discussed in detail in Section 3 as these are most applicable for use in OECT devices.
Herein, we set out three common device applications for n-type OSC materials and their requirements for high electron transport properties, namely organic thin film transistors (OTFT), organic electrochemical transistors (OECT) and organic thermoelectric generators (OTE).
Typically, the performance of an OSC for OTFT applications is judged by the mobility determined directly from operating thin-film transistors. There is no standardised OTFT architecture for the testing of new OSC materials, as is clear from Tables 1–7. In an OTFT, current through the OSC is modulated by a gate electrode with a dielectric layer between it and the OSC. In practice, the materials used for this dielectric and its position relative to the source and drain electrodes (staggered vs. coplanar) and above or below the OSC layer (top-gate or bottom-gate) varies. Fig. 5(a) and (b) show examples of a typical staggered, top-gate and coplanar bottom-gate OTFT configuration, which are the predominant configurations used to test the OSCs discussed here. Contact engineering, choice of dielectric, OTFT configuration and device optimisation play a large role in dictating the electrical characteristics of an OTFT and thereby the mobility extracted.
Polymer | EAb (eV) | M n/Mw (kDa) | Max. μe (cm2 V−1 s−1) | I ON/IOFF | V T (V) | Channel L/W (μm) | Device structure | Ref. |
---|---|---|---|---|---|---|---|---|
Where multiple testing conditions are detailed in literature, the best electron mobility is reported in the table above.a Where values aren’t reported directly in the text, these are inferred from given transfer plots.b EA is an estimation of the LUMO, although neglects the electron binding energy. | ||||||||
P(NDI2OD-T2) | 3.91 | 26.6/85.1 | 6.40 | 107 | <10 | 20/2000 | St.TG; Au – PMMA/Al | 95 |
PNDIF-T2 | 4.01 | 28/57 | 3.93 | 105 | 14 | 150/1500 | St.BG; SiO2/OTS – Au | 53 |
P(NDI2HD-T2) | — | 97.8/244.5 | 1.90 | >104 | 35 | 50/1000 | St.BG; SiO2/OTS – Au | 96 |
P(NDI2SiC6-T2) | 3.83 | 32/65 | 1.04 | 103 | 22 | — | St.TG; Au – PMMA/Al | 101 |
PNBSF | 3.88 | 56.1/238.2 | 3.50 | — | 48 | 5/1400 | St.TG; SiO2/Au/OTS/PFBT – PMMA/Al | 62 |
PNBS | 3.81 | 39.7/147.6 | 0.29 | >103 | 42 | 5/1400 | Co.BG; SiO2/Au/OTS/PFBT | 62 |
PNBTF | 3.85 | 48.5/221.6 | 2.20 | >103 | 60 | 5/1400 | St.TG; SiO2/OTS/Au/PFBT – PMMA/Al | 62 |
PNBT | 3.77 | 36.7/148.6 | 3.20 | >103 | 38 | 5/1400 | St.TG; SiO2/Au/OTS/PFBT – PMMA/Al | 62 |
PNDIF–TVT | 3.99 | 33/51 | 3.75 | 105 | 15 | 150/1500 | St.BG; SiO2/OTS – Au | 53 |
PNDI–TVT | 4.00 | 139/70 | 1.80 | 106 | 13 | 10/1000 | St.TG; Au/Cs2CO3 – PMMA/Al | 52 |
P3 | 4.00 | 18.6/63.5 | 0.50 | 105 | 15 | 50/500 | St.TG; Au – PMMA/Au | 102 |
PNDIBS | 3.90 | 106.5/40.1 | 0.24 | 106 | 12 | 100/1000 | St.BG; SiO2/OTS – Au | 103 |
pSNT | 4.01 | 61.3/153.3 | 5.35 | >106 | 1 | 100/1000 | St.TC; SiO2/OTMS – Au | 104 |
P4 | 4.02 | 54.9/98.8 | 7.16 | >106 | 1 | 100/1000 | St.TC; SiO2/OTMS – Au | 105 |
Polymer | EAb (eV) | M n/Mw (KDa) | Max. μe (cm2 V−1 s−1) | I ON/IOFF | V T (V) | Channel L/W (μm) | Device structure | Ref. |
---|---|---|---|---|---|---|---|---|
Where multiple testing conditions are detailed in literature, the best electron mobility is reported in the table above.a Where values aren’t reported directly in the text, these are inferred from given transfer plots.b EA is an estimation of the LUMO, although neglects the electron binding energy. | ||||||||
PNDTI-BT-DT | 4.40 | 27.1/90.4 | 0.27 | >102 | 10 | 40/3000 | St.BG; SiO2/OTS – Au | 106 |
PNDTI-BT-DP | — | 149.6/16147.0 | 0.24 | >105 | 13 | 40/1450 | St.BG; SiO2/MAPS – Au | 110 |
PNDTI-BTT-DP | 4.40 | 20.5/51.9 | 0.31 | >105 | 4 | 40/1500 | St.BG; SiO2/OTS – Au | 58 |
PNDTI-NTz | 4.20 | 15.7/27.2 | 0.21 | >104 | 15 | 40/1500 | St.BG; SiO2/OTS – Au | 59 |
PDNTI-BTz | 4.10 | 14.4/42.2 | 0.10 | 104 | 20 | 40/1500 | St.BG; SiO2/OTS – Au | 59 |
Polymer | EAb (eV) | M n/Mw (kDa) | Max. μe (cm2 V−1 s−1) | I ON/IOFF | V T (V) | Channel L/W (μm) | Device structure | Ref. |
---|---|---|---|---|---|---|---|---|
Where multiple testing conditions are detailed in literature, the best electron mobility is reported in the table above.a Where values aren’t reported directly in the text, these are inferred from given transfer plots.b EA is an estimation of the LUMO, although neglects the electron binding energy. | ||||||||
BDPPV | 4.24 | 37.6/89.4 | 1.10 | >105 | 5 | 10/200 | St.TG; SiO2/Au – CYTOP/Al | 87 |
BDOPV-2T | 4.15 | 77.2/231.5 | 1.74 | >104 | 44 | 5/100 | St.TG; SiO2/Au – CYTOP/Al | 86 |
AzaBDOPV-2T | 4.37 | 51.6/135.0 | 3.22 | >104 | 40 | 5/100 | St.TG; Au – CYTOP/Al | 60 |
F4BDOPV-2T | 4.32 | 38.0/109.1 | 1.56 | >103 | 3 | 100/2000 | St.TG; SiO2 – CYTOP/Al | 85 |
Polymer | EAb (eV) | M n/Mw (kDa) | Max. μe (cm2 V−1 s−1) | I ON/IOFF | V T (V) | Channel L/W (μm) | Device structure | Ref. |
---|---|---|---|---|---|---|---|---|
Where multiple testing conditions are detailed in literature, the best electron mobility is reported in the table above.a Where values aren’t reported directly in the text, these are inferred from given transfer plots.b EA is an estimation of the LUMO, although neglects the electron binding energy. | ||||||||
PAIIDBT | 4.10 | 14.0/22.0 | 1.00 | 106 | 30 | 20/1000 | St.TG; Au – PMMA/Al | 64 |
PIIG-BT | 3.54 | 15.0/19.8 | 0.22 | >107 | 48 | 50/1000 | St.BG; SiO2/OTS – Au | 65 |
P6F-C3 | 3.80 | 52.9/81.5 | 4.97 | >106 | 55 | 80/5600 | St.TG; SiO2/Au – PMMA/Au | 115 |
P6F-2TC3 | 3.92 | 88.0/170.7 | 1.35 | 106 | 45 | 80/5600 | St.TG; SiO2/Au – PMMA/Au | 115 |
2FIID-BT2CN | 3.92 | 111.0/170.9 | 0.25 | >104 | 10 | 80/5600 | St.TG; SiO2/Au – PMMA/Al | 116 |
Polymer | EAb (eV) | M n/Mw (kDa) | Max. μe (cm2 V−1 s−1) | I ON/IOFF | V T (V) | Channel L/W (μm) | Device structure | Ref. |
---|---|---|---|---|---|---|---|---|
Where multiple testing conditions are detailed in literature, the best electron mobility is reported in the table above.a Where values aren’t reported directly in the text, these are inferred from given transfer plots.b EA is an estimation of the LUMO, although neglects the electron binding energy. | ||||||||
BTI1-DPP | 3.34 | 24/— | 0.27 | >104 | 16 | 5000/20000 | St.TGC; Au/CsF – CYTOP/Al | 119 |
BTI2-DPP | 3.42 | 23/— | 0.48 | >104 | 27 | 5000/20000 | St.TG; Au/CsF – CYTOP/Al | 119 |
BTI3-DPP | 3.46 | 21/— | 0.21 | >105 | 18 | 5000/20000 | St.TG; Au/CsF – CYTOP/Al | 119 |
PPyTDPP-TT | 3.75 | 120.0/352.0 | 0.48 | >106 | 64a | 50/4500 | St.TG; Au – PMMA/Al | 120 |
pTPDPP-TF | 4.10 | 24.4/125.3 | 0.10 | 104 | 14 | 20/1000 | St.TG; Au – PMMA/Al | 88 |
PPyDPP1-4FBT | 3.65 | 157.4/291.2 | 1.02 | 105 | 28 | 80/5600 | St.TG; SiO2/Au – PMMA/Al | 121 |
PPyDPP2-4FBT | 3.69 | 120.2/271.7 | 2.45 | 105 | 25 | 80/5600 | St.TG; SiO2/Au – PMMA/Al | 121 |
PPyDPP1-4FTVT | 3.66 | 102.7/181.8 | 1.19 | 106 | 15 | 80/5600 | St.TG; SiO2/Au – PMMA/Al | 121 |
PPyDPP2-4FTVT | 3.67 | 126.2/214.5 | 1.35 | 106 | 21 | 80/5600 | St.TG; SiO2/Au – PMMA/Al | 121 |
DPPTh-BT2CN | 3.67 | 155.0/207.7 | 0.35 | >103 | 15 | 80/5600 | St.TG; SiO2/Au – PMMA/Al | 116 |
DPPPy-BT2CN | 3.75 | 275.0/357.5 | 0.30 | >104 | 1 | 80/5600 | St.TG; SiO2/Au – PMMA/Al | 116 |
Polymer | EAb (eV) | M n/Mw (kDa) | Max. μe (cm2 V−1 s−1) | I ON/IOFF | V T (V) | Channel L/W (μm) | Device structure | Ref. |
---|---|---|---|---|---|---|---|---|
Where multiple testing conditions are detailed in literature, the best electron mobility is reported in the table above.a Where values aren’t reported directly in the text, these are inferred from given transfer plots.b EA is an estimation of the LUMO, although neglects the electron binding energy. | ||||||||
P4 | 4.20 | 134/538 | 0.2 | >102 | 18 | 20/1000 | St.TG; Au – PMMA/Al | 68 |
BBL | 4.00 | — | 0.03–0.10 | — | — | 25/500 | Co.BG; SiO2/HMDS/Au | 51 |
P(BTimR) | 3.47 | 12.7/27.1 | 3.71 | 106 | 25 | 50/5000 | St.TG; Au/CsF – CYTOP/Au | 124 |
PCNI-BTI | 3.78 | 26.2/36.7 | 0.13 | 104 | 35 | —/5000 | St.TG; Au – CYTOP/Al | 125 |
PDTzTI | 3.77 | 7.3/7.7 | 1.61 | >107 | 24 | 50/— | St.TG; Au – CYTOP/Al | 89 |
Polymer | EAb (eV) | M n/Mw (kDa) | μ e (cm2 V−1 s−1) | I ON/IOFF | V T (V) | Channel L/W (μm) | Device structure | Ref. |
---|---|---|---|---|---|---|---|---|
Where multiple testing conditions are detailed in literature, the best electron mobility is reported in the table above.a Where values aren’t reported directly in the text, these are inferred from given transfer plots.b EA is an estimation of the LUMO, although neglects the electron binding energy. | ||||||||
PPPyr-Cl | 4.00 | 15.6/23.4 | 3.40 | 20 | 8.4 | 10/10000 | Co.BG; SiO2/Au/HMDS | 130 |
PBFI-T | 3.80 | 47.5/174.8 | 0.30 | >105 | 25 | 100/1000 | St.BG; SiO2/OTS8 – Ag | 10 |
PDIC8-EB | 3.90 | 66.9/282.3 | 0.10 | 20 | 8 | 40/800 | Co.BG; SiO2/Au/HMDS | 131 |
PIDOBT-TT | 4.13 | 37.8/88.8 | 0.29 | 105 | 9 | 80/5600 | St.TG; Au/Ba(OH)2 – PMMA/Al | 132 |
PIDOTT-TT | 4.03 | 28.6/64.6 | 0.38 | 105 | 8 | 80/5600 | St.TG; Au/Ba(OH)2 – PMMA/Al | 132 |
PIDOTT-BT | 4.05 | 19.8/46.1 | 0.45 | 105 | 5 | 80/5600 | St.TG; Au/Ba(OH)2 – PMMA/Al | 132 |
In n-type OTFTs, misalignment of the workfunction of the source and drain electrodes with the LUMO level of the OSC results in a barrier to electron injection into/extraction from the n-type OSC.90 As the LUMO of OSCs varies, it is therefore difficult to directly compare if the transport properties of the OSC itself have been improved by structural modifications or simply the charge extraction from the material in the device. To facilitate electron injection, such barriers must be minimised, which can be done by careful selection of the source/drain contact material or the addition of self-assembled monolayers (SAMs) at the interface.91,92 Surface modifications are also employed to reduce charge trapping and enhance the order of the n-type OSCs when deposited. By improving the interfaces within the OTFT, mobility is maximised.93 The minimum gate voltage required to fill trap states and produce mobile charge carriers is the threshold voltage (VT).
Fig. 5(b) illustrates the operation of an n-type OTFT, where a positive gate bias (Vg) is applied, polarising the dielectric layer and resulting in the formation of a thin interfacial electron accumulation layer in the OSC, through which a drain current (ID) flows when a voltage is applied between the source and drain electrodes (Vd). The OTFT Id as a function of Vg at constant Vd, is referred to as the transfer characteristics, and from these, mobility can be determined in either the linear (Vd < Vg − VT) or saturation (Vd ≥ Vg − VT) regime (eqn (1) and (2)), where the mobility is dependent on channel length (L), width (W) and dielectric capacitance (C).83 Importantly, this mobility is not the intrinsic mobility of the OSC on which the OTFT is based and typically mobilities determined in the saturation regime are higher.
(1) |
(2) |
Tables 1–7 present the performance of OSCs in n-type OTFTs for which an electron mobility >0.1 cm2 V−1 s−1 has been reported, specifically where the electron mobility significantly dominates over any hole mobility also reported. In these tables, the OTFT architecture and channel lengths used are summarised to put in context the values of mobility extracted from the OTFTs. The values stated in this review are the highest reported for each material in literature, irrespective of testing conditions or device architecture and geometry. The values have not been normalised and non-ideal output characteristics have not been accounted for or discussed.
The comparison of P(NDI2HD-T2) and P(NDI2OD-T2) (Fig. 6) considers the impact of sidechain engineering on the performance of the polymer, whilst retaining the same NDI-T2 polymer backbone. The performance of N2200 was improved upon by changing the sidechains for a shorter branched alkyl alternative, reducing the number of carbons in the chain by four, to give P(NDI2HD-T2), which resulted in a 50% increase in the highest reported mobility for N2200 at the time (1.22 cm2 V−1 s−1), to achieve a mobility of 1.90 cm2 V−1 s−1 (Table 1).96 This simple structural change caused the microstructure to become significantly more crystalline, with a much higher melting enthalpy than N2200, comparable to that of highly crystalline P3HT.97,98 This trend continues when comparing the π–π stacking distance, which shortens as the alkyl chain length is decreased. These combined factors result in a significant increase in the mobility recorded for P(NDI2HD-T2) through a simple sidechain modification.
Fig. 6 Chemical structures of reported OTFT polymeric materials containing NDI derivatives, including their published synonyms. |
The second NDI series for comparison is PNBSF, PNBS, PNBTF and PNBT (Fig. 6), where PNBSF is the highest performing n-type material of the series, with good stability in air (Table 1).62 Two polymers, PNBT and PNBTF contain the more traditional thiophene heterocycles flanking the benzothiazole (BT) unit, while the remaining three comprise selenophene moieties. The introduction of a selenium atom brings with it the improved orbital overlap induced by the larger p-orbital, which can facilitate improved electron transport, as such both selenium-containing polymers have higher electron mobilities than those containing thiophenes (Fig. 4).99,100 This is due to the enlargement of the heteroatom orbitals moving down the group, which becomes decreasingly well matched with the size of the neighbouring carbon orbitals, worsening orbital overlap, increasing the quinoidal character of the molecule and the energy of the double bond. Furthermore, the selenophene unit introduces excellent film-forming abilities, which can be rationalised through the enhanced interchain heteroatom–heteroatom interactions, possible due to the larger size of selenium orbitals.62,99 Another clear extension to this design strategy is the transition from a standard BT unit, to a difluorinated BT unit, which causes a transition from ambipolar transport properties of PNBS and PNBT to the unipolar electron transport exhibited by PNBSF and PNBTF (Fig. 6). Fluorination results in a deepening of the LUMO, which can lead to improved operational stability in air.62 The introduction of selenium and fluorine atoms does however add synthetic and processing challenges, where the particularly strong intermolecular interactions create solubility issues, limiting them to processing in hot chlorobenzene, while PNBT is readily soluble at room temperature in most chlorinated solvents.62
Whilst P(NDI2SiC6-T2) does not exhibit a particularly notable electron mobility (1.04 cm2 V−1 s−1; Table 1), the chemical design provides an interesting discussion point, as it demonstrates a hybrid material which exhibits advantages of both organic and inorganic properties.101 The selected sidechain constitutes an alkyl spacer, capped with a siloxane group, which enables the polymer morphology to be controlled through variation of the solvent, likely due to solubility induced pre-aggregation. For example, casting a film of P(NDI2SiC6-T2) from chloroform results in a mixed edge-on and face-on orientation, whilst casting from 1-chloronaphthalene produces a film that is almost exclusively edge-on, with a much more amorphous microstructure.101P(NDI2SiC6-T2) only displays an out-of-plane (010) π–π stacking reflection in the grazing incidence X-ray diffraction (GIXD) pattern when cast from chloroform, so these interactions cannot be quantified for the exclusively edge-on microstructure. This is supported by the improved electron mobility for the chloroform cast films (1.04 cm2 V−1s−1) when compared to the 1-chloronaphthalene cast films (which has a maximum mobility of 0.85 cm2 V−1 s−1).101 Having this control of the microstructure of a polymer, and therefore the charge carrier mobility, simply through changing the processing solvent and conditions, is an attractive proposition.
The concept of modifying the sidechain to alter the microstructure of the material is further demonstrated with PNDIF-T2, where a semifluoroalkyl sidechain is utilised.53 These sidechains offer strong self-organisation on account of the fluorophobic interactions commonly found in heavily fluorinated molecules, which creates large areas of crystallinity and long-range order, as evidenced by the GIXD pattern which shows a well-defined (h00) peak up to the fifth order for the out-of-plane direction and a prominent (010) reflection for the in-plane direction. This coexisting face-on and edge-on arrangement is created by the rigid polymer backbones and is reflected in the impressive electron mobility of 3.93 cm2 V−1 s−1, with good stability in air (Table 1).53
Polymers PNDIF–TVT, PNDI–TVT and P3 all employ a thienylene–vinylene–thienylene (TVT) electron rich comonomer unit, which is thought to extend the conjugation length of the monomer unit and contribute to improved crystallinity of the backbone (Fig. 6).52,53,102 Whilst these polymers are not a comparable series due to the multiple variables, it can be noted that the TVT comonomer appears to deepen the LUMO compared to the T2 moiety, likely due to the extension of the conjugated unit, with these polymers all offering EAs of 4 eV (Table 1). The final two NDI derivatives for discussion are pSNT and P4, the latter of which exploits the vinylene group to enhance backbone planarity (shown by DFT calculations) through interactions of the vinyl protons with the carbonyl oxygen on the NDI unit.105 This, combined with the benzobisthiadiazole (SN), results in a remarkable electron mobility of 7.16 cm2 V−1 s−1.105
The NDI derivatives are the largest class of electron transporting OTFT materials and offer some clever design solutions to ensure unipolar transport and overcome amorphous microstructures, with many NDI derivatives displaying stability in air. The main design strategies considered here are those of heteroatom substitution62,84 with the aim of improving LUMO delocalisation across the entire polymer backbone rather than its typical localised state on the electron deficient monomer, and sidechain engineering to shorten the sidechain96 or introduce halogen atoms to improve the crystallinity of the microstructure through better π–π stacking and self-organisation of the material.53
The first chemical design point to note here is the structure of PNDTI-BT-DP compared to PNDTI-BT-DT,110 and PNDTI-BTT-DP, compared to PNDTI-BTT-DT (Fig. 7), where each of the pair has the same structure aside from an extra carbon before the branch point of the sidechains. In both cases, this has the effect of pushing the alkyl chains further from the polymer backbone, and increases the electron mobility, for example PNDTI-BTT-DP shows a three-fold increase from 0.096 cm2 V−1 s−1 of PNDTI-BTT-DT to 0.31 cm2 V−1 s−1 (Table 2).58 This can be explained by examining the polymers with X-ray diffraction (XRD), which shows an in-plane π–π stacking peak for PNDTI-BTT-DP, whereas this is not present for PNDTI-BTT-DT. Notably, PNDTI-BTT-DT also displays a broad peak assignable to out-of-plane π–π stacking, indicating there may be some face-on orientation in this film, which disrupts the crystalline order of the microstructure and worsens the electron mobility.58
Fig. 7 Chemical structures of reported OTFT polymeric materials containing NDTI derivatives, including their published synonyms. |
The other comparison with these relatively high performing NDTI derivatives is between PDNTI-BTz and PDNTI-NTz (Fig. 7).59 These polymers present the same NDTI unit and sidechains, with the distinguishing feature being the comonomer as either benzo[c][1,2,5]thiadiazole (BTz) or naphtho[1,2-c:5,6-c′]bis[1,2,5]thiadiazole (NTz). In the reporting of this polymer series, other comonomers were used, however they either produced low performance (vinylene), or ambipolar polymers (thienylenevinylene and naphtho[1,2-b:5,6-b′]-dithiophene).59 It was initially thought that the use of a smaller comonomer, such as vinylene, would be advantageous in promoting the orbital overlap with the LUMO, allowing it to delocalise more than usual. However, this picture was not validated, as the largest comonomer actually exhibits the highest mobility (Table 2). This, as before, can be explained by examining the GIXD pattern, where PDNTI-NTz has the most crystalline structure, clearly displaying both an edge-on orientation and in-plane π-stacking.59
NDTI derivatives have not yet outperformed the heavily studied NDI derivatives. The underlying design principle with these polymers is to increase the backbone rigidity and create polymers with more long-range order and larger regions of crystallinity, but this remains to be demonstrated.
Fig. 8 Chemical structures of reported OTFT polymeric materials containing polylactam/lactone derivatives, including their published synonyms. |
The next polymer in the series, AzaBDOPV (Fig. 8), builds on this D–A polylactam/lactone derivative and incorporates an additional nitrogen into the polylactam/lactone core, transforming the phenyl into a pyridine derivative.60 These sp2 nitrogen atoms create a more electron deficient acceptor unit, which increases the EA to 4.37 eV (Fig. 4). This facilitates electron injection, increases the mobility by two-fold to 3.22 cm2 V−1 s−1 in ambient conditions and unsurprisingly, it also removes the observation of ambipolar transport for this material (Table 3).60 The final polymer, F4BDOPV-2T (Fig. 8), also aims to improve on BDOPV-2T with the introduction of two fluorine atoms on the phenyl rings.85 These have the dual purpose of both reducing the electron density of the polylactam/lactone core and increasing the planarity of the backbone via further intramolecular non-covalent short contacts between one fluorine atom and a proton on the bithiophene unit, and the strong non-covalent F–S interaction. These interactions can be visualised by examining the phenyl–thienyl dihedral angle, which decreases from 21.9° in BDOPV-2T, to 9.6° in F4BDOPV-2T.85 This must be on account of the interactions because the fluorine atom itself has an atomic radius that is almost 25% larger than hydrogen.112 These combined effects increase the EA to 4.32 eV (Table 3).
The strategic design surrounding these polylactam/lactone derivatives include introducing an electron-donating comonomer (typically bithiophene), utilising electron-withdrawing functionalities (such as fluorine atoms appended to85 or nitrogen atoms embedded into the backbone)60 to deepen the LUMO of the polymer and improve electron injection, and focussing on how to create backbone planarity through intramolecular interactions, including non-covalent short contacts (Fig. 4). Due to the electron deficient backbones, and in turn the low-lying LUMOs of polylactam/lactone derivatives in this series, they all produce air-stable n-type devices, with some of the highest mobilities reported for electron transporting OTFTs.85
The lowest performing of the isoindigo polymers reported in Table 7, PIIG-BT, was reported alongside PIIG-TPD, which displays the same IIG core and sidechains, and a thienopyrroledione comonomer unit (Fig. 9).65 The mobility improvement for PIIG-BT compared to PIIG-TPD is explored by examining the polymers with atomic force microscopy (AFM), where both films formed densely interconnected nanofibrillar domains, with the grains in PIIG-BT over double the size of those in PIIG-TPD.65 It is believed that this gives PIIG-BT higher electron mobilities, owing to the ability of the material to form much larger crystalline domains.65
Fig. 9 Chemical structures of reported OTFT polymeric materials containing isoindigo (IIG) derivatives, including their published synonyms. |
PIIG-BT is then further improved by mimicking the approach taken with the polylactam/lactone polymers, through the introduction of nitrogen atoms into the phenyl rings, to form PAIIDBT, which results in the IIG unit becoming more electron deficient and increasing the EA from 3.5465 to 4.10 eV,64 leading to a five times increase in mobility (Table 4). The difference with this design approach however, is that these materials are an acceptor–acceptor (A–A) copolymer, constituting two electron deficient monomers. This approach aims to lower the LUMO to improve ambient stability and potentially allow for more dense packing of polymer chains (Fig. 4).117 Use of A–A motifs also results in a deepening of the HOMO, increasing the energetic barrier to hole injection, bringing the potential benefit of lowering OTFT off-currents.89 The use of traditional D–A copolymers is a well-established synthetic plan to improve performance, however the relatively new field of A–A copolymers is still worth studying for the prospect of developing high performing n-type OTFT materials.
The first series compares BTI1-DPP, BTI2-DPP and BTI3-DPP (Fig. 10), whereby the BTI unit extends in length by fusing another BTI unit through the terminal thiophene.119 With each additional BTI unit, the electron acceptor character increases, and the EA increases to 3.46 eV for BTI3-DPP, from 3.34 eV for BTI1-DPP, however backbone planarity is compromised, with the dihedral angle increasing from ∼3° to 10°, as predicted by DFT calculations.119 The highest electron mobility is observed for BTI2-DPP (0.48 cm2 V−1 s−1; Table 5), where there is a careful balance between deepening the LUMO sufficiently to support electron injection and ensuring planarity of the backbone is maintained.119
Fig. 10 Chemical structures of reported OTFT polymeric materials containing diketopyrrolopyrrole (DPP) derivatives, including their published synonyms. |
To assess the influence of the comonomer, the sidechain length and the branching position on n-type performance, a series of four DPP polymers incorporating fluorine atoms were investigated, namely PPyDPP1-4FBT, PPyDPP2-4FBT, PPyDPP1-4FTVT and PPyDPP2-4FTVT (Fig. 10).121 All polymers exhibit electron mobilities above 1.0 cm2 V−1 s−1, with the highest performing, PPyDPP2-4FBT, presenting μe of 2.45 cm2 V−1 s−1 (Table 5).121 All polymers show stronger (100) and (200) diffraction peaks by GIWAXs than the non-fluorinated derivative, indicating a higher crystallinity in these materials, which accounts for the impressive electron mobilities. Furthermore, fluorination decreases the π–π stacking distances, from 3.59 Å for PPyDPP1-BT, to 3.56 Å for PPyDPP1-4FBT.121
The final DPP comparison is that of DPPTh-BT2CN and DPPPy-BT2CN, whereby the flanking units around the DPP are altered from thiophene to pyridine motifs, to investigate the impact on the LUMO level and the electron mobility (Fig. 10).116 These, combined with electron-withdrawing cyano functionalities on the T2 comonomer, ensure the LUMOs are deep enough to support n-type behaviour, resulting in electron mobilities of 0.35 and 0.30 cm2 V−1 s−1 respectively (Table 5).116 Whilst DPPTh-BT2CN displays a low hole mobility, the pyridine derivative suppresses hole injection completely through increasing the ionisation potential (IP, which is an approximation of the HOMO energy level) from 5.41 to 5.83 eV.116 This wide selection of DPP polymers clearly shows that this moiety has application in n-type OTFT materials, despite not offering particularly high EAs.
Fig. 11 Chemical structures of reported OTFT polymeric materials containing an acceptor–acceptor (A–A) motif, including their published synonyms. |
The fused polymer, BBL, has recently been a pioneering material in the fields of n-type OECTs and OTEs. In OTFTs, an electron mobility of 0.1 cm2 V−1 s−1 has been achieved, which has been attributed to the close π-stacking of the fused backbone (3.51 Å).51,126 Thin films of BBL have been shown to contain crystalline domains on the order of 50–125 nm and this crystallinity has been suggested to act as a kinetic barrier to prevent oxygen diffusion into the films, thereby enhancing the stability of OTFTs based on BBL.127
Another A–A example are polymers containing the thiazole imide moiety. Whilst the fused thiophenes of the thiazole imide motif, shown in Fig. 11 as P(BTimR), PCNI-BTI and PDTzTI, are electron-rich units, the strongly electron-withdrawing imide group overrides the monomer to give it an electron accepting character. The simplest of the series is P(BTimR), which contains only a single repeat unit and exhibits a high electron mobility of 3.71 cm2 V−1 s−1.124 This material, however, exhibits a low EA of 3.47 eV, severely limiting the ambient stability. PDTzTI has been synthesised to include thiazole motifs, increasing both the EA and IP. However, the EA remains relatively low at 3.77 eV, which still limits the ambient stability of these devices.89,128 Cyanation is an effective way to deepen the LUMO level of OSCs, and in this case a series of cyanated P(BTimR) derivatives were demonstrated to effectively increase the EA from 3.47 to 3.78 eV, though this was still not fully effective to sufficiently improve ambient stability and did not increase μe,max (Table 6).125
Fig. 12 Chemical structures of a selection of the remaining unclassified n-type OTFT polymeric materials, including their published synonyms. |
PPPyr-Cl (Fig. 12) demonstrates a cationic backbone structure which affords a high EA of 4.00 eV and an impressive μe,max of 3.40 cm2 V−1 s−1 (Table 7). High gate voltages are required to obtain these mobilities (15–20 V) whereas mobilities at a gate voltage of 5–15 V are 0.24 cm2 V−1 s−1.129,130 The approach of utilising a water-soluble ionic structure remains interesting for application in transistors, and could potentially also see uses in OECT devices.
Another polymer which provides a novel design strategy is PDIC8-EB, due to its employment of alkyne linkers between the two comonomers (Fig. 12). Without these, the phenyl–phenyl linker has a low quinoidal character and would result in a high degree of twisting along the backbone, reducing crystallinity and electron transport properties. The introduction of the linear alkyne group supports the predisposition of perylene diimide (PDI) units to π-stack, which results in a reasonable OTFT μe of 0.1 cm2 V−1 s−1 (Table 5).131
The final series for discussion utilises a novel thienoquinoidal unit flanked with isatin groups. This unit is either in a bithiophene or thienothiophene type arrangement, and coupled with T2 or TT in a D–A motif to present the polymers PIDOBT-TT, PIDOTT-TT and PIDOTT-BT (Fig. 12).132 This design strategy employs a sulfone group, which forces a single isomeric structure due to the steric hinderance of the many oxygens in close proximity. These polymers have high EAs above 4.0 eV, resulting in good air stability and reasonable electron mobilities, with the highest performer, PIDOTT-BT, recording 0.45 cm2 V−1 s−1 (Table 7).132 This can be explained by the planarity of the backbone of this polymer, which has continuously been found to relate to the order of the thin films. Due to the fused nature of the TT unit in the centre of the acceptor monomer of PIDOTT-BT, this monomer has a dihedral angle of 0° by X-ray diffraction, enabling short π–π stacking distances of 3.45 Å.132 This novel series proves that whilst there is significant focus in the field on optimising pre-existing polymeric materials, there are still alternatives yet to be discovered that offer reasonable OTFT performance.
The n-type OSCs applied to OECTs are mixed conductors which allow for electron transport along their conjugated backbones and ionic transport through the bulk of the material (Fig. 13(a)). In an n-type OECT operating in accumulation mode, the current between the source and drain electrodes is modulated by changes in the effective gate bias, which causes an injection of electrons into the volume of the channel, followed by a migration of ions into the bulk OSC layer (Fig. 13(b)). This migration of ions is controlled by either an immersed electrode in the OECT electrolyte or biomolecular activity changing ion gradients in the electrolyte.135
The mixed conduction of both electrons and ions by the n-type OSC means that charge transport cannot be modelled in the same way as in OTFTs. One of the first theories developed to model the operation of OECTs was Bernards’ model, which simultaneously applies an electronic and ionic circuit to treat OECTs operating in depletion mode, as opposed to accumulation mode.135 Non-uniform charge carrier densities across the channel, contact resistance, swelling of the polymer film on operation and polaron binding energies are further considerations which are taken into account by more developed models.136
For OECTs, the slope of change in current as a function of gate bias (eqn (3)), referred to as the transconductance, gm, is commonly used to compare the properties of OECTs.39,137
(3) |
A metric more relevant to the transport properties of the n-type OSC itself, rather than the OECT device, is the product of mobility (μ) and capacitance of the channel per unit volume (C*). This so called [μC*] product considers the device geometry, effective gate voltage (Vg) and threshold voltage (VT) of the OECT. Using eqn (4), [μC*] can be determined from the OECT transconductance.
(4) |
In some cases, the [μC*] product has been decoupled ([μ][C*]) by determining mobility through time of flight or impedance spectroscopy measurements. A similar trend in [μC*] derived directly from OECTs and [μ][C*] calculated from independent μ and C* measurements has been demonstrated, though in general, the calculated [μ][C*] product is underestimated relative to the [μC*] product.137 Every technique for determining the mobility of disordered OSCs will give slightly different values due to the nature of the systems under investigation and the measurement itself. This discrepancy between some material measurements and the actual application of the device can lead to an overinflation of how useful a material is.
Exposure of OSCs to aqueous electrolyte has been shown to result in the migration of water molecules as well as ions into the film, causing it to swell. The magnitude of this swelling is dependent on the chemical structure and morphology of the OSC and a greater degree of swelling results in a higher volumetric capacitance and thereby increased transconductance.141,142 Whilst swelling is beneficial for efficient uptake of ions by the OSC at low operating voltages, excessive OSC swelling has been shown to have a detrimental effect on mobility,143 as the crystallinity of the microstructure is disrupted and so the number of pathways for charge transport throughout the polymer are reduced.133
Through sidechain engineering, changing the ratio of alkyl and glycol sidechains enables the NDI-T2 polymer backbone to be tailored to two-dimensional OTFT operation or to optimum OECT operation with three-dimensional charge transport (Fig. 14).142 This n-type backbone, with all alkyl sidechains, performs well in OTFT devices, but its hydrophobicity inhibits its ability to operate as the mixed transport layer in an OECT. By introducing a controlled ratio of glycol chains, i.e. an alkyl/glycol sidechain random copolymer, ionic transport can be facilitated, allowing the polymer to operate as an OECT, when the percentage of glycol chains reaches 75% (Fig. 14).142 The optimal ratio for this backbone was found to be 90% glycol and 10% alkyl sidechains, resulting in the polymer, P-90.142P-90 is favoured for use with enzymes, such as the work with glucose oxidase (GOx), which requires a suitable surface interaction between the OSC and the enzyme.146 It has been observed that the enzyme adsorption on the surface of the thin film is quite sensitive to the 90% glycol ratio, demonstrating that the sidechains not only impact the performance of a material in OECTs, but also affect the devices potential applications based on interactions with the desired biological media.
Fig. 14 The molecular structures of the all alkyl OTFT material (P-0) and all glycol OECT material (P-100) and schematic illustrations of their operation. Cations are depicted in blue, anions in white and electrons throughout the polymer backbone are grey. Adapted from literature.80,142 |
The particular difficulty with electron transporting OECT materials is their requirement to operate in ambient conditions, meaning their electron polaron must be stable to oxygen and water. As previously stated (Fig. 2), a deep LUMO level is required to aid stability, as well as a low threshold voltage to ensure the device operates at its optimum performance within applied voltage range of 0.89 to −1.23 V, to avoid the oxidation of water or the reduction of oxygen respectively.81
Whilst a material can be inherently ambipolar, it has been observed that when sweeping the voltage in one direction to achieve one type of charge transport, then sweeping in the opposite direction, the stability of the material in both directions is limited upon repeating the cycling. Mitigation against this degradation can be achieved by suppressing hole injection with a low-lying HOMO.4,147,148
Taking the figures of merit discussed in Section 3.1 into consideration, it is quite clear that a material can be deemed high performing based on a number of different parameters. These materials fall into two main categories: naphthalenediimide (NDI) derivatives (Fig. 15),142 and fully fused A–A polymeric backbones (Fig. 16), in both cases building on conjugated backbones widely utilised in polymers designed for n-type OTFTs.7,149 The key properties and common figures of merit for a comprehensive selection of OECT n-type polymers are set out in Table 8.
Fig. 15 Chemical structures of reported OECT polymeric materials containing NDI derivatives, including their published synonyms. |
Fig. 16 Chemical structures of reported OECT polymeric materials utilising a fully fused acceptor–acceptor derivatives, including their published synonyms. |
Material | EAa (eV) | M n/Mw (kDa) | μ e (cm2 V−1 s−1) | C* (F cm−3) | [μC*] (F cm−1 V−1 s−1) | g m′g (S cm−1) | Ref. |
---|---|---|---|---|---|---|---|
a EA is an estimation of the LUMO, although neglects the electron binding energy. b These EA values were measured by subtracting the optical bandgap from the IP (measured by PESA). c These EA values were measured with cyclic voltammetry in 0.1 M TBAPF6 acetonitrile solution, using the onset of reduction to calculate the EA. d Method of obtaining this range was unspecified. e These molecular weight values were determined by GPC. f These molecular weight values were determined by MALDI-TOF. g g m′ represents the thickness normalised transconductance; where this was not explicitly reported, it has been calculated by dividing the transconductance by the thickness. | |||||||
P-90 | 4.23b | 7.8/12.4e | 2.38 × 10−4 | 198 | — | 0.210 | 142 |
P-100 | 4.17b | 7.2/9.0e | 1.96 × 10−4 | 192 | — | 0.204 | 142 |
p(NDI-T2-L2) | 4.50b | Not reported | — | 95 | 0.31 | 0.520 | 150 |
p(gNDI-gT2) | 4.12c | 16.8/50.1e | 1.00 × 10−5 | 397 | — | 1.085 | 81 and 151 |
p(C3-gNDI-gT2) | 4.10c | 32.4/73.5e | — | 72 | 0.13 | 0.34 | 151 |
p(C6-gNDI-gT2) | 4.00c | 20.2/54.1e | — | 59 | 0.16 | 0.37 | 151 |
p(C2-T2) | 4.10b | 18.8f | 3.97 × 10−4 | 492 | 0.20 | 0.40 | 152 |
p(C4-T2) | 4.10b | 11.3f | 1.90 × 10−3 | 158 | 0.30 | 0.63 | 152 |
p(C6-T2) | 4.20b | 25.0f | 4.74 × 10−3 | 272 | 1.29 | 2.28 | 152 |
p(C8-T2) | 4.20b | 14.9f | 3.76 × 10−4 | 342 | 0.13 | 0.15 | 152 |
BBL | 4.00d | Not reported | 2.14 × 10−3 | 731 | 1.99 | 0.815 | 126 |
PgNaN | 4.28c | 20.7/162.1e | 6.50 × 10−3 | 100 | 0.66 | 0.212 | 149 |
PgNgN | 4.35c | 8.7/19.3e | 1.89 × 10−4 | 239 | 0.04 | 0.007 | 149 |
As in the case of OTFTs, optimisation of polymer processing and introducing n-type dopants have delivered enhanced OECT performance, for example, solvent engineering has been shown to increase transconductance by up to three-fold.156 Films of P-90 are typically spin-cast from pure chloroform (pristine film), however one study utilised chloroform with increasing percentages of acetone, from 5–20 vol%, with peak performance observed at 15% acetone to give a [μC*] product of 0.057 F cm−1 V−1 s−1 (from 0.0188 F cm−1 V−1 s−1).156 This is explained by an altering of the morphology due to a change in solubility of the polymer induced when introducing a poorer solvent (acetone), which causes larger regions of the films to be crystalline, due to greater aggregation in the solution. Above 15% acetone, it is thought that the solution became too aggregated, resulting in films with a high degree of crystallinity, which then hinders efficient ion transport due to a lack of amorphous regions.156 Another approach to boost the amplification ability of P-90 based OECTs encompasses the use of the n-dopant, tetra-n-butylammonium fluoride (TBAF).154 Doping had not been utilised in n-type OECT materials, and with an optimal addition of 40 mol% of the dopant, this method has provided not only an extremely impressive gm′ of 0.910 S cm−1 but also good stability, with no changes to peak current or transconductance when pulsed at 0.5 V for 4.5 hours.154
Further studies have been carried out to examine the effect of using a hybrid sidechain, composed of both aliphatic and ethylene glycol motifs.151,152 The first of these studies takes the high performing material p(gNDI-gT2) and introduces an alkyl spacer between the NDI unit and the ethylene glycol chain in order to reduce detrimental swelling properties observed upon doping. This strategy is verified by comparing the C* values of the original p(gNDI-gT2) polymer (221 F cm−1) with the propyl and hexyl spacer materials (72 and 59 F cm−1; p(C3-gNDI-gT2) and p(C6-gNDI-gT2) respectively; Table 8 and Fig. 15).151 As expected, when the hydrophobic alkyl content is increased in these materials, the C* value decreases on account of fewer ions being stored by the polymer, as determined by Electrochemical Quartz Crystal Microbalance with Dissipation (EQCM-D).151 This reduced swelling also contributes to a more stable current response, with no decline in the current when switching on and off for 2 hours for p(C6-gNDI-gT2) at the gate voltage where peak transconductance is measured (0.6 V), which proves useful for practical application in bioelectronic devices.151 The study reports that no accurate values could be obtained for the electron mobilities of these materials due to the low currents observed, however the increase in the [μC*] product observed when lengthening the alkyl spacer from zero (0.06 F cm−1 V−1 s−1) to six (0.16 F cm−1 V−1 s−1) implies that electron mobility must be increasing.151
The second spacer study utilises a similar approach, aiming to find the optimum alkyl spacer length for highest OECT performance, varying the spacer length from C2 to C8 (namely p(C2-T2), p(C4-T2), p(C6-T2) and p(C8-T2)) (Fig. 15).152 The OECT performance, measured by both gm′ and [μC*], increases from p(C2-T2) (0.40 S cm−1) through to p(C6-T2) (2.28 S cm−1) then drops for the octyl spacer unit (Table 8). As speculated in the previous study, the electron mobility here is observed to increase with alkyl spacer length, peaking for the hexyl spacer unit, and explaining the trend seen both with the [μC*] product and normalised transconductance, which presents p(C6-T2) as the current highest performing n-type OECT material based on both transconductance and [μC*].152 This is due to the increase in long-range order through the formation of more interconnected crystalline regions.152 These design strategies remain relatively straightforward and prevent the need for a random three component polymer, such as P-90, to control levels of swelling and optimise morphology to maximise performance.
A recent study which compared materials, BBL and P-90, managed to improve on the previously high gm′ value of ∼0.6 S cm−1 with an increase of one third, to realise a gm′ of 0.815 S cm−1.126 It should be noted that the key difference in this study compared to the original work with BBL in OECT devices is the processing method, which was originally spray coating, and in this work utilised a spin-coating deposition method.7,126 This emphasises the importance of selecting the appropriate processing conditions to maximise the performance of a material. This work also produced a [μC*] value of 1.99 F cm−1 V−1 s−1, which further highlights the impact of a sidechain-free structure.126 By conducting ex situ GIWAXS measurements, it could be seen that the coherence lengths, which are reflective of the order in the film, increased upon electrochemical doping by 9% for BBL. In contrast, coherence lengths for P-90 after doping reduced by 15%, showing a decrease in order in the film.126 This was also verified by examining the π-stacking distances, which is already shorter in BBL (3.51 Å, compared to 3.82 Å in P-90) and further contracts upon doping, which is likely beneficial for charge transport.126
However, as a result of the lack of sidechains, processing of BBL requires aggressive conditions, such as methanesulfonic acid. One particular area where BBL requires improvement is the response time, which is expectedly slow (∼1 s) on account of the limited diffusion of ions throughout the active layer.7,8
The concept of a fully fused polymer backbone was further investigated with the recent publication of PgNaN and PgNgN (Fig. 16), which builds on OTFT polymers P3, P4 and P5 (Fig. 11) by substituting the alkyl sidechains with glycol sidechains.149 Here, the materials were designed to achieve a near torsion-free π-conjugated backbone with an A–A configuration (Fig. 4). This electron deficient structure led to very high EA values of 4.28 and 4.35 eV respectively, and high performing OECT n-type mobilities of up to 6.50 ± 1.01 × 10−3 cm2 V−1 s−1 (Table 8), on account of the very well delocalised LUMO orbitals,36 surpassing the previous best performing OECT material, BBL, by an order of magnitude. Perhaps even more notably both PgNaN and PgNgN are synthesised via a metal-free aldol condensation polymerisation, an acid catalysed coupling absent of any toxic metals, common to most polymerisations, a major benefit for potential bioelectronic or sensing applications.144
The two polymers differ only by the composition of the sidechains, with PgNgN offering a fully glycolated backbone, whilst PgNaN displays a 50:50 ratio of alkyl to glycol sidechains. Yet this is enough to have a significant impact on performance, with the all glycol derivative showing a [μC*] value an order of magnitude lower than that of the mixed alkyl/glycol derivative. This is similar to the trend observed by the NDI series including P-90 and P-100,142 again indicating that incorporation of some alkyl sidechains aids OECT performance, likely due to the ability of alkyl chains to modulate swelling of OECT materials.143 The use of an alkylated monomer, to form PgNaN, benefits both solubility and processability leading to an increase in polymer molecular weight.149 Therefore, to decisively state whether PgNaN is higher performing due to its incorporation of alkyl sidechains, polymers of the same molecular weight should be compared.
The fused structure of these rigid rod-like polymers prevents twisting due to the double bond which locks the conformation of connecting monomer units, minimising disorder and trapping sites, optimising charge transport along the backbone.7,51 Coupled with the highly electron-deficient acceptor–acceptor configuration these fused glycolated polymers are a promising new class of high performing OECT materials.
Other design strategies for improving OECT performance including planarising the backbone utilising carbon–carbon double bonds to “lock” the conformation,149 increasing the electron deficiency of the repeat units,81 and replacing the traditional donor–acceptor moiety142 for an acceptor–acceptor backbone to deepen the LUMO and facilitate electron injection.149
σ = qnμ | (5) |
PF = S2σ | (6) |
(7) |
Limitations of n-type dopants include their redox stability and the immiscibility of the oxidised species with the OSC as well as the adverse impact on OSC morphology by disrupting packing.70,169,170 The inherent instability of n-dopants has limited the development of n-type OTE materials compared with their p-type counterparts. The very shallow dopant HOMO levels required to n-type dope OSCs mean air stable n-dopants are rare, as possessing such a low IP increases the dopants susceptibility to oxidation by ambient species.45 For efficient n-type doping of OSCs, a deep OSC LUMO level below −4.0 eV is required.66
There is a slim selection of n-dopants for application in OTEs, including tetrakis(dimethylamino)ethylene (TDAE),171 4-(1,3-dimethyl-2,3-dihydro-1H-benzoimidazol-2-yl)-N,N-dimethylaniline (N-DMBI)172 and triaminomethane (TAM) (Fig. 18(a)).170TDAE is not air stable, and therefore has limited applications in OTEs. N-DMBI is one of the most commonly used and best understood n-type dopants for OTE materials, likely due to the ambient stability of the native species.66,172,173 Stability of N-DMBI and TAM as n-type dopant precursors originate from the mechanism of doping, which is via a latent hydride (formed in situ) or an initial hydrogen removal, rather than simply donating an electron, meaning requirements of the n-type dopant to have a low IP are alleviated.154,170,172 When using N-DMBI, the resulting cation has exhibited poor miscibility with typical alkyl substituted n-type OSCs, one rationale for investigating more polar sidechains.174
Fig. 18 (a) Four n-type dopants commonly used in OTE applications, their neutral ambient stabilities and the ability of the cations to assist in the doping process, (b) a schematic representation of the doping of FBDPPV with N-DMBI and with (c) TAM.170 |
TAM is the state-of-the-art n-dopant as it maintains the excellent n-doping abilities of N-DMBI, whilst improving its miscibility with alkylated polymers, meaning n-type OTEs can benefit from the catalogue of pre-existing polymers developed for n-type OTFT applications. TAM enables uniform doping, with minimal effect on the π–π stacking of polymer backbones, as demonstrated with n-type polymer FBDPPV (Fig. 20).170 This occurs as the TAM+ cation has a small molecular volume and remains in the sidechain region due to a weak affinity with the π-backbones and a stronger affinity with the polymer sidechains, due to compatibility with its own cyclic alkyl sidechains.167 Conversely N-DMBI typically moves into the π-backbone region to avoid incompatible polarities between the dopant molecule and the alkyl sidechains, as predicted by statistical analysis of equilibrium-state counterion-backbone distances.170 This can be explained by DFT calculations, which predict that TAM+ has a stronger affinity with alkyl sidechains due to the respective polarizabilities of the dopant and the sidechain region, thus enabling TAM+ to pack more tightly than N-DMBI during doping (Fig. 18(b) and (c)).
Another approach in the direction of air-stable n-type dopants is the use of organometallic dimers with high reducing abilities.175 These are able to cleave in situ, which is followed by a rapid electron transfer to the OSC. The n-dopant, (pentamethylcyclopentadienyl)(1,3,5-trimethylbenzene)ruthenium ([RuCp*Mes]2), is particularly impressive as it has a very shallow HOMO, so is able to dope polymers with LUMOs as shallow as −2.8 eV (Fig. 18(a)).176
Thermal stability of the doped n-type OSC is key, especially for thermoelectric applications. Films of OSCs doped with N-DMBI exhibited poor thermal stability, with the observed loss of σmax attributed to de-doping.177 Good thermal stability was observed in another study sequentially doping with N-DMBI, that is doping the thin film rather than solution of the OSC.178 Improved thermal stability when using N-DMBI has also been observed when there is good miscibility between the polymeric OSC and dopant, for example when polar side chains are used.70 Adequate miscibility between the polymer and dopant enables a uniform distribution of dopant molecules within the polymer matrix, limiting aggregation and ultimately doping a greater proportion of the polymer, enhancing TE performance.179 This was corroborated by a recent study comparing the doping efficiency and resultant thermoelectric performance of the dimeric (N-DMBI)2 dopant (which forms the same N-DMBI+ cation as N-DMBI, without involving a hydrogen atom or hydride transfer) against the (RuCp*mes)2 dopant (Fig. 18(a)) for FBDPPV containing OTE devices.180 These results suggest that, at least for the doping of ordered polymers, molecular dopants should be designed to have a more planar shape to minimise perturbation of ordered microstructures and to facilitate efficient electron-transfer reaction pathways.
It is clear that the dopant and its interactions with the n-type OSC are vital to maintaining a stable value of σmax under prolonged thermal stress. This discussion highlights that the choice of dopant can be considered equally important as the n-type OSC material itself, making comparison between new materials difficult and rational design of n-type OSCs for OTEs is restricted by and often relies upon the available dopants.
Fig. 19 Chemical structures of selected n-type thermoelectric NDI polymer derivatives, including published synonyms. |
Fig. 20 Chemical structures of selected n-type thermoelectric polylactam/lactone derivatives, including published synonyms. |
Polymer | EAa (eV) | M n/Mw (kDa) | Dopant | σ max (S cm−1) | PF (μW m−1 K−2) | Ref. |
---|---|---|---|---|---|---|
a EA is an estimation of the LUMO, although neglects the electron binding energy. b These molecular weight values were determined by GPC. c This molecular weight value was determined by MALDI-TOF. | ||||||
N2200 | 3.90 | Not reported | N-DMBI | 0.008 | 0.6 | 187 |
TEG-N2200 | 3.96 | 3.8/4.6b | N-DMBI | 0.2 | 0.4 | 181 |
p(gNDI-gT2) | 4.10 | 8.8c | N-DMBI | 0.3 | 0.4 | 174 |
P(NDI2OD-Tz2) | 4.10 | 32.2/54.7b | TDAE | 0.1 | 1.5 | 171 |
PNDI2TEG-2Tz | 4.26 | 26.2/29.7b | N-DMBI | 1.8 | 4.5 | 189 |
An alternative approach is to replace the bithiophene (T2) unit of N2200 with a bithiazole (Tz2) moiety, affording P(NDI2OD-Tz2) (Fig. 19), a polymer with improved π–π stacking due to reduced intrachain steric demands in Tz2 versus T2, leading to greater backbone planarity.171 The increased electron-deficient character of Tz2 increases the EA and decreases the D–A character (Fig. 4), resulting in a σmax of 0.1 S cm−1 (Table 9), rising by two orders of magnitude compared to N2200 also doped with TDAE (Fig. 18; 0.003 S cm−1).159,187
The benzodifurandione-based polymer (BDPPV) exhibits a high EA value of 4.0 eV and forms part of a series with ClBDPPV and FBDPPV (Fig. 20). These polymers introduce halogen atoms, which increase the EA by 0.3 and 0.17 eV respectively, improving doping efficiency and more than doubling electron mobility, compared to BDPPV (Table 9).66 This can be attributed to the electron-withdrawing and planarizing effects of including pendant fluorine atoms, which act as a conformational lock through intrachain non-covalent short contacts to minimise the dihedral angle about the double bond between the lactone and isatin moiety. As a result, upon doping with N-DMBI both ClBDPPV and FBDPPV show increased σmax and PF compared to unhalogenated BDPPV. Further improved PF values of 51 μW m−1 K−2 were reported for FBDPPV by incorporating the newly-developed n-dopant TAM (Fig. 18).68 The original BDPPV polymer backbone was further modified through glycolation, replacing one alkyl chain with an OEG chain to furnish UFBDPPV (Fig. 20). Upon doping with TAM, a very impressive OTE performance was reported, with σmax of 22.5 S cm−1 and a PF of 80 μW m−1 K−2.167 The increased σmax of UFBDPPV is due to the highly miscible TAM cations which do not disturb the polymer microstructure and enable an efficient interchain charge transport in the conductive films. The asymmetric sidechain distribution of UFBDPPV allows for this amphipathic polymer to benefit from both excellent dopant-polymer miscibility, whereby dopant molecules are confined to the hydrophilic sidechain region, whilst retaining good π–π packing thus increasing doping efficiency and σmax.190 The benefit of including OEG-based sidechains for positive polymer-dopant interactions has been corroborated through multiple studies and has been proven as an effective method for increasing OTE performance.174,180,181,191
The inherent instability of n-type materials drove interest in blocking the polymer backbone from contact with oxygen and water during device operation.192 As such, building upon the previous BDPPV-based polymers, a difluoro- and dichloro-substituted form of the electron-deficient BDOPV unit were coupled with the relatively weak donor moiety dichlorodithienylethene (ClTVT), resulting in two D–A BDOPV-based polymers, PClClTVT and PFClTVT, designed to minimise backbone contact with ambient species (Fig. 20).67 Despite the two polymers sharing an identical backbone, the replacement of chlorine with fluorine atoms on the electron-deficient BDOPV unit has a remarkable influence on the σmax, which is rationalised with the same explanation as for the BDPPV polymer series. Indeed, σmax of PClClTVT is 16.1 S cm−1, which is less than half that of PFClTVT (38.3 S cm−1), furthermore the PF of PFClTVT reached 22.7 μW m−1 K−2, three times that of PFClTVT (Table 10).67 Once again, the drastically improved σmax and resultant TE performance of both these materials, particularly PFClTVT, are dominated by the charge carrier mobility, following eqn (5). It should also be noted that the authors reported that PClClTVT, doped with 50 mol% N-DMBI, retained a σmax value of 4.9 S cm−1 after storing in air for 222 days, a very considerable stability for an n-doped polymer stored in air.67
Polymer | EAa (eV) | M n/MwMn/Mwb (kDa) | Dopant | σ max (S cm−1) | PF (μW m−1 K−2) | Ref. |
---|---|---|---|---|---|---|
a EA is an estimation of the LUMO, although neglects the electron binding energy. b Molecular weight values were determined by GPC. | ||||||
BDPPV | 4.01 | 41.8/99.9 | N-DMBI | 0.3 | 1.6 | 66 |
ClBDPPV | 4.30 | 38.6/97.3 | N-DMBI | 7.0 | 16.5 | 66 |
FBDPPV | 4.17 | 42.9/101.2 | N-DMBI | 14.0 | 28.0 | 66 |
UFBDPPV | 4.13 | 34.5/122.8 | TAM | 22.5 | 80.0 | 167 |
PClClTVT | 4.00 | 58.6/130.6 | N-DMBI | 16.1 | 7.6 | 67 |
PFClTVT | 4.03 | 39.4/140.6 | N-DMBI | 38.3 | 22.7 | 67 |
Fig. 21 Chemical structures of selected n-type thermoelectric NDTI polymer derivatives, including published synonyms. |
Polymer | EAa (eV) | M n/Mwb (kDa) | Dopant | σ max (S cm−1) | PF (μW m−1 K−2) | Ref. |
---|---|---|---|---|---|---|
a EA is an estimation of the LUMO, although neglects the electron binding energy. b Molecular weight values were determined by GPC. | ||||||
pNB | 4.20 | 11.5/18.4 | N-DMBI | 0.01 | 0.3 | 107 |
pNB-Tz | 4.22 | 11.6/22.0 | N-DMBI | 0.9 | 9.9 | 107 |
pNB-TzDP | 4.22 | 15.4/35.4 | N-DMBI | 11.6 | 53.4 | 107 |
PDTzTI | 3.80 | 7.2/7.7 | TDAE | 4.6 | 7.6 | 184 |
PNDTI-BTT-DT | 4.40 | 17.6/83.4 | N-DMBI | 0.12 | 0.6 | 58 |
PNDTI-BTT-DP | 4.40 | 20.5/51.9 | N-DMBI | 5.0 | 14.2 | 58 |
Although the BTI unit imparts a wave-line backbone for the pNB polymer, as predicted by DFT calculations,107 a BTI homopolymer, PDTzTI, (Fig. 21) exhibits a near coplanar backbone with enhanced crystallinity.89 Moreover, closer π–π stacking and A–A character further improved charge carrier generation and transportation compared to pNB. As a result, PDTzTI achieved a notable σmax of 4.6 S cm−1 and a PF of 7.6 μW m−1 K−2 (Table 11).184
Fig. 22 Chemical structures of selected n-type thermoelectric DPP polymer derivatives, including published synonyms. |
Polymer | EAa (eV) | M n/Mwb (kDa) | Dopant | σ max (S cm−1) | PF (μW m−1 K−2) | Ref. |
---|---|---|---|---|---|---|
a EA is an estimation of the LUMO, although neglects the electron binding energy. b Molecular weight values were determined by GPC. | ||||||
P(TDPP-CT2) | 3.70 | 34.0/73.0 | N-DMBI | 0.4 | 9.3 | 182 |
P(PzDPP-CT2) | 4.03 | 28.5/82.8 | N-DMBI | 8.4 | 57.3 | 182 |
PDPH | 3.93 | 30.9/75.4 | N-DMBI | 0.001 | 0.0005 | 186 |
PDPF | 4.11 | 29.9/75.6 | N-DMBI | 1.3 | 4.7 | 186 |
Polymer | EAa (eV) | M n/Mwb (kDa) | Dopant | σ max (S cm−1) | PF (μW m−1 K−2) | Ref. |
---|---|---|---|---|---|---|
a EA is an estimation of the LUMO, although neglects the electron binding energy. b Molecular weight values were determined by GPC. | ||||||
BBL | 4.00 | Not reported | TDAE | 2.4 | 0.43 | 159 |
N–N | 3.94 | 80/215 | N-DMBI | 0.65 | 3.2 | 63 |
A–N | 3.83 | 139/480 | N-DMBI | 0.26 | 1.6 | 63 |
A–A | 3.72 | 51/162 | N-DMBI | 0.018 | 0.25 | 63 |
LPPV-1 | 4.49 | 15.8/42.2 | TAM | 4.0 | 34.8 | 196 |
In a series of three fully fused polylactams (Fig. 23), reducing the central acene core size resulted in progressively increasing EA values (Fig. 4), leading to an increasingly more favourable and efficient n-type doping with N-DMBI. Specifically, reducing the central lactam core from two anthracenes (A–A) to mixed anthracene–naphthalene (A–N) and finally to two naphthalene cores (N–N) yielded a more delocalised electron polaron and a larger EA of 3.94 eV for the N–N polymer (Fig. 23). The benefits of contracting the acene core were further substantiated by the increased TE performance, with N–N displaying the highest σmax (0.65 S cm−1) and PF (3.2 μW m−1 K−2) of the series.63
Fig. 23 Chemical structures of selected n-type thermoelectric fully fused polymer derivatives, including published synonyms. |
In LPPV-1 (Fig. 23),196 an isoindigo derivative with a coplanar rigid backbone, the central fused carbon–carbon double bond in addition to the intramolecular non-covalent short contacts between the phenyl hydrogen and adjacent oxygen atom renders the backbone near torsion free. The acceptor–acceptor character, electron-deficient lactone core, and the incorporation of electron-withdrawing moieties within the backbone led to an extremely high EA of 4.5 eV, desirable for n-doping (Fig. 4). Indeed, upon doping with N-DMBI, σmax of 1.1 S cm−1 and a PF of 1.96 μW m−1 K−2 were achieved. Akin to UFBDPPV (Table 10), the TE performance of LPPV-1 was also improved drastically upon doping with TAM, reaching σmax of up to 4.0 S cm−1 and a PF of 34.8 μW m−1 K−2 (Table 13).167 This investigation suggests that, without sacrificing Seebeck coefficients, high conductivities can be realised with precise regulation of the interaction between the cations and the host. Ultimately both the intrinsic polymer performance parameters (planarity, LUMO level, mobility) and the interaction between polymer and dopant must be optimised to maximise OTE performance.
This review also addresses the challenges in extracting comparable data, including variations in how measurements are conducted, differing device architectures and lack of clarity or overinflation when reporting numbers.
Despite the variance in device architectures, the improved structure–performance properties published by multiple research groups tend to follow similar trends which include; judicious use of electron deficient units to deepen LUMO energy levels,60,66,85 extending conjugation,36,58,59,149 maximising molecular weights,14,15,21 and altering polymer backbone electronic configuration, for example by employing an acceptor–acceptor motif.64,197,198 The material systems represented throughout, are evidence of the viability of invoking multiple different design principles to improve the performance of n-type materials towards three different fields of organic electronics, namely OTFTs, OECTs and OTEs. The recent acceleration of research and development has been rewarded with the performance of n-type materials that are beginning to approach performance seen in their p-type counterparts.
Potential directions for future work include employing strategies to maximise capacitance without compromising processability (as seen for BBL),7 methods to increase the molecular weight of glycolated polymers to improve mobility, and finding novel methods for improving stability of both n-type materials and n-dopants.170
The area of organic n-type materials continues to expand and with promising molecular design concepts to explore, the future of the field is extremely promising.