Zhiliang
Wang‡
ab,
Yu
Qi‡
ab,
Chunmei
Ding
a,
Dayong
Fan
ab,
Guiji
Liu
ab,
Yongle
Zhao
ab and
Can
Li
*a
aState Key Laboratory of Catalysis, Dalian Institute of Chemical Physics, Chinese Academy of Sciences, Dalian National Laboratory for Clean Energy, The Collaborative Innovation Center of Chemistry for Energy Materials (iChEM), Zhongshan Road 457, Dalian, 116023, China. E-mail: canli@dicp.ac.cn
bUniversity of the Chinese Academy of Sciences, Beijing, 100049, China
First published on 16th March 2016
Charge separation is one of the most critical factors for generating solar fuels via photoelectrochemical water splitting, but it is still not well understood. This work reveals the fundamental role of charge transfer in photoanodes for achieving high charge separation efficiency. Specifically, we fabricated a particulate Ta3N5 photoanode by a bottom-up method. By improving the charge separation with refined necking treatment, the photocurrent is increased by two orders of magnitude. The charge separation efficiency (ηsep) is analyzed by dividing it into charge generation efficiency (Φgene) and transportation efficiency (Φtrans). Necking treatment is found to substantially improve the electron transfer. Transient photovoltage (TPV) measurements based on the Dember effect is used to confirm the benefit of necking treatment in improving the charge transportation. The superior electron transfer in the necked-Ta3N5 electrode is further evidenced by the facile electron exchange reaction with the ferri/ferrocyanide redox couple. Moreover, cobalt phosphate is found to promote both charge separation and surface reaction, resulting in a photocurrent of 6.1 mA cm−2 at 1.23 V vs. RHE, which is the highest response for a particulate photoanode.
In PC, an efficient charge separation in particles can usually lead to fast reaction at the semiconductor/liquid interface with the assistance of a suitable cocatalyst.7 In PEC, however, photogenerated electrons must transfer through the film and be collected by the substrate to match the surface reaction. Thus, the charge transportation in the films also plays a fundamental role in the whole PEC process,8 and the interfaces of particle–particle (PP) and particle–substrate (PS) are critically important for charge transportation. To ensure good connections at these interfaces, semiconductor is usually epitaxially grown on a conductive layer in situ by, for instance, hydrothermal,9 chemical bath,10 and vapour deposition methods.11,12 Electrodes of low-dimensional structure13,14 or host–guest structure15,16 are intentionally designed to improve the charge transportation efficiency in the electrode so as to decrease the electron–hole recombination. However, most previous researches focus on charge transfer in the semiconductor particles since it determines the generation of separated electron–hole pairs,17–19 and little attention has been paid on clarifying the charge transfer process in the film, which also plays a determinable role during the photoelectrochemical reaction.
Transient photovoltage (TPV) can provide direct insight into the charge transfer process through the electrode. Upon illumination, Dember photovoltage is generated20 which stems from the diffusion difference of photogenerated electrons and holes. Typically, the gradient distributed light in the film excites photogenerated electron–hole pairs in gradient concentration21,22 which will cause them to diffuse from a high concentration region (surface, high light intensity) to the low concentration region (bulk, low light intensity) at different velocities. Then the electron–hole pairs drift apart and electric field builds up; the decay process of the photovoltage can reveal the charge transfer process in the film.
Cyclic voltammetry (CV) in the dark can also reveal the electron transfer in electrodes.23 For the cathodic reaction, electrons must transfer through the films before exchanging with an efficient redox couple, e.g. Fe(CN)63−/Fe(CN)64−. The magnitude of the cathodic current and potential of the reduction peak can reveal the electron transportation in the film. In addition, a particulate electrode with well-connected film can result in porous structure which provides a large electrochemical surface area for reaction. This area is proportional to the capacitance of the Helmholtz layer which can be determined from CV24 and so we can evaluate the charge transportation in the film by an electrochemical method.
Suitable materials and fabrication methods of the electrodes are important for us to pinpoint the issue of charge transportation. In terms of materials, semiconductors with long free paths are the best candidates because it permits us to focus on the charge transfer at the PP interfaces regardless of the charge diffusion in the semiconductor crystals. Ta3N5 is reported to have a diffusion length of ∼103 nm,25 indicating a long life time of photogenerated charges. Moreover, Ta3N5 has demonstrated an outstanding photocatalytic oxygen evolution activity,26 indicating an effective charge separation in Ta3N5 crystals. Also, the excellent light harvesting ability of Ta3N5 makes it an appealing material for photoelectrochemical water splitting with a potential solar energy conversion efficiency of 15% under AM 1.5 G sunlight.27 For the fabrication of the electrode, a bottom-up method, that is by depositing as-prepared semiconductor particles on the conductive substrate to form a particulate electrode, can make it more facial so as to regulate the charge transfer at the PP and PS interfaces without influencing the intrinsic properties of the semiconductor such as light absorption, carrier concentration etc. Electrophoretic deposition (EPD) method is an alternative choice. A wide range of semiconductors can be fabricated into electrodes with controllable thickness by EPD, such as Fe2O3,28 BiVO4,29 Ta3N5,30 TaON,31,32 while post-necking treatment has been found to be powerful in improving the PEC response.30–34 Some explanation to the possible function of necking treatment has been proposed,31 but more stringent evidences are required to identify the effects of this modification.
Herein, we take Ta3N5 as a demonstration to show the influence of charge transportation on the PEC performance of a particulate Ta3N5 electrode. By optimizing the substrate, precursor concentration, temperature of necking treatment and cocatalyst loading, we have achieved the highest photocurrent for electrodes fabricated by EPD. The TPV based on Dember photovoltage and CV measurements are used to clarify the critical effect of necking treatment on charge transfer at the interfaces of particle–particle and particle–substrate.
The photocurrent was recorded under simulated light (AM 1.5 G, 100 mW cm−2) at a scan rate of 50 mV s−1 from −0.8 V to 0.6 V vs. SCE in 1 M NaOH aqueous solution (pH 13.6).
The incident photon-to-current conversion efficiency (IPCE) was measured under monochromatic light irradiation provided by a tungsten lamp equipped with a monochromator (CROWNTECH, QEM24-D 1/4 m Double).
Faradaic efficiency was tested by recording the photocurrent and the generated O2 simultaneously. The O2 evolution was evaluated by gas chromatography (GC, Agilent 7890a GC) with a 5 Å molecular sieve column. Argon carrier gas with a velocity of 10.0 mL min−1 was used to purge the working electrode compartment to carry the evolved gases to GC for analysis. The quantity and retention time of the gases were calibrated with a series of standard gas samples.
All the (photo)electrochemical tests were conducted on an Ivium potentiostat/galvanostat in a three-electrode system with a quartz window. A piece of platinum foil (2 cm × 2 cm) was used as counter electrode and saturated calomel electrode (SCE, 0.241 V vs. RHE) used as the reference electrode. The potential was converted to the reversible hydrogen electrode (RHE) scale by the Nernst equation as below:
E(RHE) = E(SCE) + 0.059pH + 0.241 | (1) |
Despite the small changes of the morphology of Ta3N5 particles, the PEC performance shows a substantial difference with necking treatment (Fig. 2a). The raw-Ta3N5 electrode exhibits notoriously low photoresponse, and so does the TaCl5 treated electrode. However, after necking treatment, the photocurrent of the necked-Ta3N5 electrode increases to 1.56 mA cm−2 from 9 μA cm−2. For the necking treatment, the TaCl5 concentration and post-heating temperature have great influence on the photoresponse of the necked-Ta3N5 electrode (Fig. S3†). The optimized TaCl5 concentration is 15–20 mM (concentration at 20 mM gives the best repeatability) and the best post-heating temperature is 600 °C for the refined necking treatment. At high temperature, the particles will have strong connection with each other at the PP and PS interfaces. However, NH3 has strong capability of reduction at high temperature, and can damage the normally used FTO substrate.28,31 Some metal based candidates were chosen and Ti foil gave the best result (Fig. S4†). The benefit of calcination is also confirmed by the improved photoresponse of heated-Ta3N5 compared to the raw-Ta3N5 electrode. Further cocatalyst loading, e.g. CoPi,39 on necked-Ta3N5 electrode efficiently accelerates the water oxidation to an optimized current of 6.1 mA cm−2 at 1.23 V vs. RHE (Fig. 2b), which is higher than most reported results fabricated by the EPD method.30,31,40,41 In Fig. 3, IPCE action spectra show the quantum efficiency at different irradiation wavelengths, which are in agreement with the absorption of Ta3N5. The raw-Ta3N5 electrode shows very low IPCE, but after the refined necking treatment, it dramatically increases to more than 20%. Also, the IPCE is much higher by loading CoPi or increasing the bias to accelerate the consumption of photogenerated charges.
Fig. 3 IPCE of raw-Ta3N5 (orange), necked-Ta3N5 (black) and CoPi/necked-Ta3N5 (red) electrodes. The absorption spectrum (black solid curve) for raw Ta3N5 is presented for comparison. |
The refined necking treatment plays a key role in boosting the photoanodic performance of the particulate Ta3N5 electrode and it is also essential for the cocatalyst functioning Ta3N5 photoanode. Thus we endeavour to pinpoint the exact role of necking treatment by analysing the reaction at the semiconductor/liquid interface and charge transfer at PP and PS interfaces on the particulate Ta3N5 electrode.
For an electrode made from powder, necking treatment may have an influence on both the intrinsic property of Ta3N5 particles and the connection among particles. In order to elucidate the possible change of Ta3N5 crystals, the absorption spectra and photocatalytic activity (see ESI for details†) were measured. The absorption spectrum of Ta3N5 shows little change after necking treatment (Fig. S5a†), indicating that the necking treatment does not influence the intrinsic light harvest in Ta3N5. From the absorption spectra, the marginal photocurrent of the electrode was evaluated to be ∼12.6 mA cm−2 under simulated sunlight (AM 1.5 G, 1 sun) (Fig. S5†). The influence of necking treatment to the Ta3N5 particles were further ascertained by photocatalytic O2 evolution. In a PC reaction (Fig. 4a), light is harvested in the Ta3N5 crystal and photogenerated charges drift to the active sites to take part in the surface reaction. The proportion of photogenerated charges that reach the surface reaction sites to those generated in Ta3N5 particles upon illumination is referred as charge generation efficiency (Φgene), which is basically the charge separation efficiency in the Ta3N5 crystal. To preventing possible confusion with the separation efficiency in the electrode (as will be mentioned below), we define it as generation efficiency for the crystal. This generation efficiency is largely determined by the bulk property of the crystal. The proportion of photogenerated holes that take part in the (electro)chemical reaction to those arriving at the reaction sites is referred as injection efficiency (ηinj), which is influenced by the surface property of Ta3N5. When the surface is not preferred for catalytic water oxidation, although sufficient holes reach the reaction sites, they cannot be consumed in time and ηinj will be less than unity. In the presence of efficient electron scavengers, the influence of electrons in the crystal is limited and the PC reaction can be used to evaluate the intrinsic properties of the Ta3N5 particles, such as the charge generation in the crystals and hole injection on the surfaces.42 The PC activities of the Ta3N5 powder from the raw-Ta3N5 electrode and necked-Ta3N5 electrode were evaluated with AgNO3 as sacrificial reagent.26 As is shown in Fig. 4b, the amount of released O2 for necked-Ta3N5 has slightly decreased, implying that necking treatment has limited influence on the intrinsic property of Ta3N5.
Then we focussed on the impact of necking treatment to the electron transfer at the PP and PS interfaces in the Ta3N5 electrode. In a PEC reaction (Fig. 4a), electrons and holes should be considered simultaneously since the electrons need to transfer through the Ta3N5 films during the PEC water oxidation. The transportation of photogenerated charges will be another factor that limits the PEC performance.
As it is reported, the final photocurrent is determined by the following expression:43,44
J = J0ηLHηsepηinj | (2) |
The absorption and PC water oxidation measurement have revealed that necking treatment has little influence on light harvest (ηLH) and surface reaction (ηinj). Hence, the difference of charge separation (ηsep) of the electrode should be responsible for the huge difference of the PEC activity. Taking H2O2 as hole scavenger,43 the charge separation efficiency is calculated. From Fig. 4c, it is revealed that the charge separation in raw-Ta3N5 electrode is inefficient, but necking treatment improves ηsep to more than 30% at the bias of 1.3 V vs. RHE. Interestingly, we found that CoPi/necked-Ta3N5 electrode has an even higher ηsep of 60% at 1.3 V vs. RHE.
A higher separation efficiency means less electron–hole recombination in the electrode. For a photoelectrocatalytic reaction occurring on a particulate electrode (Fig. 4a), the recombination may occur via two routes: (i) recombination in the particles through, for example, bulk defects or surface states; (ii) recombination at the interfaces of particles. Thus the measured separation efficiency should be dependent on the charge generation in particles and transfer among particles under illumination:
ηsep = ΦgeneΦtrans | (3) |
CoPi has been reported to suppress the surface states, and more long-lived photogenerated holes can survive in the particles.46 Thus, the Φgene is increased and this leads to the cocatalyst promoted charge separation for the CoPi/necked-Ta3N5 electrode (Fig. 4c). For the necked-Ta3N5 electrode, the previous absorption (Fig. S5†) and PC activity (Fig. 4b) indicates a similar Φgene. Thus, the dramatically improved ηsep for necked-Ta3N5 electrode should stem from the improved Φtrans upon necking treatment.
To consolidate the conclusion, prototypical devices fabricated from Ta3N5 electrodes (Fig. 5a, see ESI for details†) were used to delve into the charge transportation in the electrode by TPV. In Fig. 5b, the necked-Ta3N5 based device shows higher transient photovoltage and faster decay process than the raw-Ta3N5 based device. A linear response of current-bias (Fig. S6†) confirms the ohmic contact at the interfaces of PS.20 Thus, the detected photovoltage plausibly stems from the Dember effect and this was further confirmed by the relationship between the direction of the induced laser and electric field. For the Dember effect, holes always stay closer to the top layer, and the direction of the electric field is always consistent with the direction of the laser beam (Fig. S7a†), and the intensity of the Dember voltage is determined by the amount of separated charges. Light of stronger intensity will induce more separated charges and hence a higher photovoltage (Fig. S7b†). When the intensity of the induced light is the same, and the same amount of charges are generated, a higher photovoltage indicates better charge separation. Thus the higher photovoltage of the necked-Ta3N5 device indicates that it shows better charge separation which is in accordance with the result in Fig. 4.
When light is removed, the electron–hole pairs will recombine, leading to a dynamic decay of the Dember photovoltage at the time scale of μs (Fig. 5b, solid line). Two plausible recombination processes mentioned above are involved in the decay process. Dual exponential curves (Fig. 5b, dashed line) are fitted with a fast decay process (recombination in Ta3N5 crystals, lifetime of τ1) and a slow one (recombination at interfaces, lifetime of τ2). The two electrodes have approximately the same τ1 values, confirming again that the Ta3N5 particles on both electrodes have similar charge generation efficiency (Φgene) as the PC result reveals in Fig. 4a. However, the necked-Ta3N5 electrode has lower τ2, indicating that the electron–hole pairs more readily recombine through the interfaces in the TPV devices.
In order to clarify the result of TPV further, an equivalent circuit (EC) based on the transmission line model47 (Fig. 5c) was used to simulate the decay process in the device. Because there is no semiconductor/electrolyte interface, only three processes are considered: (i) the electron transport resistance in the Ta3N5 crystals (Rcrystal), (ii) the electron transport resistance among particles (R) and particles–substrate (Rcontact), (iii) a capacitive charging to the porous Ta3N5 matrix (Cbulk). For the Ta3N5 crystal, the conduction band or the defect energy level can accommodate electrons which can behave like a capacitor (Ccrystal). Cbulk can be estimated to be at the order of 10−5 F cm−2, while Ccrystal is around 10−8 F cm−2 (see ESI for details†). Thus, Ccrystal is much smaller compared to Cbulk and the series of Ccrystal make it even smaller, so that we can ignore Ccrystal. So the equivalent circuit in Fig. 5c can be reduced to that in Fig. 5d, including the resistance among and in Ta3N5 particles. The time constant (τ′ = RbulkCbulk) of electronic decay in the simulated circuit corresponds to the lifetime (τ) determined by TPV. As the bulk capacitance (Cbulk) of the two devices (raw-Ta3N5 and necked-Ta3N5) are estimated to be of the same order of magnitude based on eqn (S1) (ESI†) the change in time constant is reflected in the change of resistance in the device. Comparing the lifetime of τ2 in the two types of Ta3N5 electrodes as tabulated in Fig. 5b, the smaller τ2 of the necked-Ta3N5 electrode means that necking treatment decreases the charge transfer resistance (Rbulk) in the Ta3N5 film.
The amorphous layer of nitrogen doped tantalum oxide that bridges the Ta3N5 particles is a plausible route for electron transportation. As necking treatment is performed at high temperature, efficient connection at interfaces of PP will be formed. Additionally, nitrogen doping in the tantalum oxide layer can improve its conductivity48 and facilitate the transportation of the photogenerated charges. Indeed, it is reasonable that low charge transfer resistance should lead to the high photovoltage and fast decay process since the Dember photovoltage is caused by drifting apart of electron–hole pairs, the better the conductivity is, the easier they can be dissociated/recombined, and vice versa.
The efficiency of electron transportation across the interfaces of PP and PS was further probed using the benchmark redox couple of ferri/ferrocyanide.23 The exchange of electrons between the solution and electrodes is fast (Fig. S8(a)†), allowing for the characterization of electron transfer by CV. The reduction reaction occurring on the Ta3N5 electrode (without illumination) can provide a direct measure on the electron transportation. In darkness, the electrochemical reduction occurs by transferring electrons from the Ta3N5 electrode to K3Fe(CN)6. Better electron transportation in the film will lead to more facial electron exchange. Moreover, the improved electron transfer in the film will decrease the ohmic polarization of the electrode and decrease the overpotential for the reduction of K3Fe(CN)6. The CV reveals that Ta3N5 is poor for hydrogen evolution (Fig. S8(b)†) but active for K3Fe(CN)6 reduction (Fig. S8(c)†). This allows us to focus on the electron exchange between the electrode and K3Fe(CN)6 regardless of the influence of hydrogen evolution in the potential window of −0.4 to 1.2 V vs. RHE. Fig. S8(c),† shows that the reduction peak of K3Fe(CN)6 shifts positively on Ta3N5 electrode, indicating that Ta3N5 is superior to Ti substrate in electrocatalytic reduction of K3Fe(CN)6. When Ta3N5 film has a good contact with the substrate, more electrons will be exchanged with K3Fe(CN)6 on the Ta3N5 particles than on the Ti substrate (Fig. S9†). Thus, the results in Fig. 6a can be related to electron transfer in the Ta3N5 film. It is found that the necked-Ta3N5 electrode has a reduction current of −19.7 mA cm−2 at 0.65 V vs. RHE, while that for the raw-Ta3N5 electrode is −18.1 mA cm−2 at 0.38 V vs. RHE, which is similar to that of the substrate (Fig. S8(c)†). The more positive potential along with higher current of the reduction peak indicates more efficient electron exchange on necked-Ta3N5 electrode. Because electrons should transport through the particulate Ta3N5 film, it is concluded that necked-Ta3N5 electrode is superior to raw-Ta3N5 electrode in electron transportation (Fig. S9†). The reduction peak potential of raw-Ta3N5 electrode (0.38 V vs. RHE) is close to the substrate (0.37 V vs. RHE), indicating that more electrons are leaked out through the substrate other than through Ta3N5 because of the weak connection at the PS interfaces. Additionally, the CV of CoPi/necked-Ta3N5 electrode is similar to that of necked-Ta3N5 electrode (Fig. S8(d)†), confirming that CoPi has little impact on the charge transfer in the electrode.
To sum up, necking treatment can facilitate charge transfer at the PP and PS interfaces in the Ta3N5 film which is beneficial for the collection of photogenerated electrons, and depressing the recombination at the interfaces.
For particulate electrode, only the particles having good connection with the conductive layer can provide the area for electrochemical reaction. If an electrode made from powder has good conductivity in the film a porous structure with large electrochemical active area is expected. By eliminating the influence of the diffusion layer with concentrated electrolyte, we can get the relative area of the electrode from its charging capacitance of the Helmholtz double layer based on the following expression:8,24
j = vC = (εS/4πd)v | (4) |
Here, we measured the charging current (j) in a potential window (−0.1 to 0.2 V vs. SCE) where there is no faradaic current at different scan rates without illumination (Fig. S10†). The j–v plot of each electrode is shown in Fig. 6b and the slope should be proportional to the surface area based on eqn (4). Taking the area of bare Ti substrate as unit, it is found the area only increases a little with TaCl5 treatment or heating. However, the refined necking treatment leads to 22 times larger electrochemical surface area. Based on the analysis above, it is inferred that for raw-Ta3N5 electrode, the poor connection in the particulate Ta3N5 layer contributes little to the electrochemical active area. Only the layer of Ta3N5 contact with the substrate can be used for reaction (Fig. S9,† left) and thus the electrochemical area is limited. After necking treatment, the connection at the interfaces of particle–particle (PP) and particle–substrate (PS) are improved substantially and even the layer of Ta3N5 far from the substrate can be used for reaction (Fig. S9,† right). Thus the necked-Ta3N5 electrode provides a much larger electrochemical surface area for reaction.
Inspired by the results above, another example was further raised to support the conclusion. We found that the necking treatment can improve the photocurrent to 6.0 mA cm−2 at 1.6 V vs. RHE for the Ta3N5 electrodes made from traditional thermal oxidation–nitridation method (Fig. S11, see ESI for details†).
As for the role of CoPi, it can improve the charge separation by enhancing the charge generation in the Ta3N5 crystal as shown above. Further, the surface charge injection process is also greatly accelerated with CoPi (Fig. S12†). Because of the cocatalyst promoted charge separation and injection, the CoPi/necked-Ta3N5 electrode can provide a photocurrent of 11.2 mA cm−2 at 1.6 V vs. RHE. Moreover, the fast consuming of photogenerated holes can protect Ta3N5 from being oxidized.44 Thus, the stability of the necked-Ta3N5 electrode is substantially improved with the assistance of CoPi as shown in Fig. 7a. The near unit faradaic efficiency of the CoPi/necked-Ta3N5 electrode (Fig. 7b) confirms that the photocurrent is originated from O2 evolution reaction. However, the photocurrent decayed noticeably with prolonged time (Fig. 7a). The failure of the Ta3N5 electrode is suspected to be the result of the large surface area of the particulate electrode which makes it difficult to wholly cover Ta3N5 with effective co-catalyst in the porous structure. Many unconsumed photogenerated holes were accumulated and destroyed the intrinsic Ta3N5. Further efforts to improve the stability is still in progress.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c6sc00245e |
‡ These authors contribute equally to this work. |