Ashley P.
Black
a,
Andrea
Sorrentino
b,
François
Fauth
b,
Ibraheem
Yousef
b,
Laura
Simonelli
b,
Carlos
Frontera
a,
Alexandre
Ponrouch
a,
Dino
Tonti
a and
M. Rosa
Palacín
*a
aInstitut de Ciència de Materials de Barcelona, ICMAB-CSIC, Campus UAB, 08193 Bellaterra, Catalonia, Spain. E-mail: rosa.palacin@icmab.es
bCELLS – ALBA Synchrotron, 08290 Cerdanyola del Vallès, Catalonia, Spain
First published on 12th December 2022
Synchrotron radiation based techniques are powerful tools for battery research and allow probing a wide range of length scales, with different depth sensitivities and spatial/temporal resolutions. Operando experiments enable characterization during functioning of the cell and are thus a precious tool to elucidate the reaction mechanisms taking place. In this perspective, the current state of the art for the most relevant techniques (scattering, spectroscopy, and imaging) is discussed together with the bottlenecks to address, either specific for application in the battery field or more generic. The former includes the improvement of cell designs, multi-modal characterization and development of protocols for automated or at least semi-automated data analysis to quickly process the huge amount of data resulting from operando experiments. Given the recent evolution in these areas, accelerated progress is expected in the years to come, which should in turn foster battery performance improvements.
Research efforts are thus on course worldwide to improve currently available battery chemistries, such as Li-ion, while at the same time looking for new concepts with high energy density and/or advantages in terms of cost and sustainability.
Batteries being intrinsically complex devices,1 mastering materials science in general, and characterization techniques in particular, is crucial to achieve progress in both research directions.
Measurements done in situ (inside the battery) or operando (taken during cell functioning) have lately boosted and improved in spectral/spatial resolution for a myriad of techniques, including diffraction and a wide spectrum of spectroscopic and imaging techniques (and even combinations thereof). Different length scales need to be probed: from Å to nm for surfaces/interfaces, and from tens of nm to μm for electrode materials, to reach mm for full electrodes and full devices.2,3 Moreover, due attention has to be paid to the sensitivity of the technique (surface vs. bulk) and to time resolution, which will determine the feasibility of mapping in dynamic processes. Beyond the use of standard state-of-the-art laboratory equipment, synchrotron radiation stands out as one of the most powerful tools within battery research.4 It allows non-destructive probing of materials with various depth sensitivities allowing fast acquisition rates, large penetration depths, high spectral or spatial resolution, and access to techniques that are only possible with a continuous tuneable source over a wide photon energy range. The use of operando techniques has intrinsic advantages, as they enable the detection of possible metastable intermediates and ensure characterization under real conditions (non-equilibrium) avoiding the risk of ex situ sample evolution during manipulation. Operando experiments are thus crucial for both the elucidation of redox mechanisms in new technologies and also understanding of failure and ageing processes for already commercial concepts, and thus their use is becoming widespread. However, compatibility between the electrochemical cell architectures and the experimental set-ups may force some specific design features and care has to be taken to ensure that these do not perturb the electrochemical response of the materials under investigation.5
Synchrotron radiation involves a wide range of photon energies. X-rays with energies above ∼4 keV are called “hard” X-rays, while those with much lower energies (and longer wavelengths) are called “soft” X-rays. The former have a larger penetration (lower absorption cross section) probing depths from a few μm to the mm range, while the latter exhibit much higher cross sections and penetration below a few μm of probing depths, being therefore much more surface sensitive. “Tender” X-rays (TX) represent an intermediate region with energies between 1 and 4 keV.
This perspective focuses on the state-of-the art of operando techniques using synchrotron radiation applied to batteries, covering from hard to soft X-rays. The first section describes the requirements for the experimental set-up, with emphasis on techniques where broader experience exists. They have been classified into three broad groups, which reflect differences in the type of radiation/matter interactions and also data analysis approaches and requirements. The second section covers techniques that are based on elastic (kinetic energy conserved) scattering, including not only diffraction (probing long range ordering) but also SAXS (Small Angle X-ray Scattering) and PDF (Pair Distribution Function), the latter providing inputs at a local scale. The third section deals with absorption or emission based spectroscopic techniques, which access the electronic structure and enable additional chemical insights: XAS (X-ray Absorption Spectroscopy) which has been well developed to perform operando experiments using hard, soft and tender X-rays and also other techniques which in this sense are less mature to date such as XPS (X-ray Photoelectron Spectroscopy) or infrared spectroscopy. The fourth section is devoted in general to imaging techniques and tomography, which, despite intrinsic physical differences, typically generate the largest datasets. Last but not least, a final Discussion and Outlook section provides the authors' view on the evolution of the field and the workarounds that may be developed in the next few years.
Fig. 1 Typical penetration depth and spatial resolution (1D and 2D measurements) for selected analytical techniques. The inset depicts 1/e penetration depths for various battery relevant materials as a function of energy (E), where e is Euler's number. TEM and SEM stand for Transmission Electron Microscope and Scanning Electron Microscope, respectively. Reproduced from ref. 6 with permission, © Materials Research Society. |
Rigid material windows ensure stack pressure and hence good electric contact. This is an often overlooked aspect, but uniform pressure is also critical for reliable electrochemical data, especially over extended cycling periods. Beryllium is the most transparent metal and widely used window, its drawbacks being high cost, toxicity and lack of stability at high potentials (becoming itself oxidized), the latter being usually alleviated by the use of an additional foil (e.g. aluminium). Yet, other thin metal foils are also an option,7 provided that absorption is not too high, or even insulating materials (glass), that can also be covered by a metal foil to enhance electronic conductivity. Note that when the same cell setup is to be employed for scattering and XAS (X-ray Absorption Spectroscopy) experiments, thin Kapton (polyimide) is used to minimize absorption, and the size of the window is often reduced to avoid decreasing stack pressure as much as possible.
In the case of SAXS (small angle X-ray scattering), some cell designs used for conventional diffraction can be used and flat cell geometry is not an issue, as the angular range is very limited and hence the X-ray path is almost identical for all scattering angles measured. The main concern is to avoid window materials which can contribute to the signal and hence materials not having long range structural order (polymers or glassy carbon) cannot be used in this case. Care has to be taken in choosing window materials not exhibiting Bragg peaks in the detector range. To this purpose, often aluminium or mica is used.
Some cell set-ups can be employed for different techniques (e.g. diffraction and XAS) and facilitate complementary studies (multi-modal characterization), while in other cases, specific geometries are required (e.g. cylindrical or radially symmetric cells for tomographic imaging). Customized cell setups were common in the early days of operando studies and new improved designs are being continuously developed8 considering adaptability to somewhat different concepts (e.g. all solid state cells). Yet, a gradual evolution to more standardized configurations has taken place,9–11 with high energy experiments allowing measurements on conventional setups (pouch, coin and cylindrical). An interesting approach to enable the use of these cells with lower beam energies is to modify them, such as laser thinning the top coin case to 50 μm. This has enabled an operando long duration ageing study for >100 cycles by simply testing the cell continuously in the beamline hutch and periodically placing it under the beam.12 Conventional setups enable improved representativity with respect to real commercial cells, but they may be limiting in some cases (e.g. spectroscopy cannot be performed unless suitable windows are implemented). Overall higher flexibility can only be achieved for specifically designed setups13–15 and can also pave the way to multimodal characterization coupling different techniques. These on purpose developed cells can allow the use of a third electrode, for independent monitoring of the potential at the positive and negative ones, opening also the possibility of performing electrochemical impedance spectroscopy on a single electrode.16 Regardless the type of cell, the high flux of synchrotron radiation allows fast data collection and thus it enables high-throughput experiments measuring multiple cells, and for this, special sample holders have been designed.13,15,17
Sample preparation is another relevant aspect, whose importance is not always emphasized.10 First of all, non-active cell components (such as binder, carbon and electrolyte) do bring in a contribution, e.g. background increase at low diffraction angles due to scattering by an amorphous carbon additive, the position of which is dependent on the electrolyte.18 Metal current collectors (typically Cu and Al for negative and positive electrodes in the Li-ion technology) will also result in sharp peaks in diffraction studies, which can mask the evolution of some overlapping peaks corresponding to the sample under study. The collector of the same element of investigation in the counter electrode is hiding the information obtainable by XAS, and a hole in the collector in correspondence with the beam path can be foreseen to avoid the overlapping signals. The total absorption of a cell (considering windows, electrodes, separator, and electrolyte) needs to be adjusted in the case of XAS measurements in transmission mode to minimize the total absorption by approaching an absorption jump of 1 for the element of interest. In particular, operando XAS at relatively low energies needs to minimize the X-ray absorption along the beam path and are often more accessible in fluorescence mode. For S K-edge operando XAS studies, for example, S compounds have been embedded in a Cu mesh to allow the penetration of the X-ray beam.19 Electrode preparation mimicking commercial protocols is a priori desirable (e.g. tape casting), as electrochemical performance will be improved. Yet, this can be a drawback for fundamental studies on the redox mechanisms of specific materials with particles exhibiting a morphology prone to preferential orientation (e.g. TiS2 platelets).18 In such a case, simple mixtures of the material with carbon black will be preferred to enable the observation of 00l reflections.
Although common battery technologies use liquid (either aqueous or organic solvent based) electrolytes, the development of batteries using solid electrolytes is currently a hot topic. Indeed, concepts involving lithium metal as the negative electrode would a priori enable very high energy densities and improved safety with respect to state-of-the-art Li-ion technology. The use of solid electrolytes brings about additional parameters to consider for operando experiments such as the need to maintain external pressure.20
Besides the control of pressure, efforts are also currently underway to extend experiments beyond ambient conditions. Their interest arises from the need to understand the influence of temperature in the redox mechanism. They can bring in relevant data regarding real battery operation under very different environments as temperature will impact kinetics and can also induce phase transitions within the electrodes. Moreover, these studies can also provide inputs on temperature driven degradation reactions. In effect, cycling to temperatures of up to 70 °C is a common means to accelerate ageing phenomena in batteries.24 Ideally, the cell designs should not differ much from those used at room temperature to ensure the representativity of the electrochemical behaviour. The main issue in this case is to be able to heat/cool the cell to a homogeneous and controlled temperature. Note that the thermal expansion of the unit cells of the materials under study does also need to be considered and that it provides a suitable indirect way to calibrate the cell temperature. While heating could be a priori easier via an electrical resistance, interference with the electrochemical response cannot be excluded. Since a crucial aspect is ensuring that the probed sample (and not only the housing) is thermalized, a circulating fluid inside the cell body appears as the most attractive option enabling both heating and cooling (Fig. 2). Other options could be to work with cylindrical cells, which could be placed inside a cryostat or a hot blower, as in this case the geometry would enable the combination with other techniques, such as tomography.
Fig. 2 Image of a thermalized cell21 designed taking the one reported in ref. 22 as the basis, modified to enable fluid circulation through the main cell body (top). Diffraction patterns achieved using a similar setup for Na3V2(PO4)2F3 in sodium cells at C/10 and 0 °C, which enabled the phase diagram to be followed upon Na+ deintercalation in 2D (a) and 3D (b) plots. Reproduced from ref. 23 with permission, © WILEY-VCH Verlag GmbH & Co. |
In addition to the generic interest in elucidating the influence of temperature in the redox mechanism, these experiments may be even more relevant in specific battery technologies operating at high temperature, such as Li metal solid polymer electrolyte cells, commercialised using LiFePO4 as the positive electrode, which operate at ca. 80 °C.25 In this case, a capillary cell setup was used, wrapped in a heating band, which enabled the control of temperature and spatially resolved phase distribution. The results allowed inferring the differences between the structural changes taking place close to the electrolyte and those occurring in the vicinity of the current collector. With respect to cooling, the study of the redox mechanism in graphite electrodes at 0 °C has also been reported, with the stage sequence observed being different from the one taking place at room temperature, which is relevant to understand the behaviour of Li-ion cells in cold climates.26 Experiments at different temperatures may also be relevant for new battery technologies, for instance, experiments down to −40 °C cooling pouch cells with liquid N2 were carried out to get further insights into the intercalation of chloroaluminate in graphite electrodes in aluminium batteries.27
Since most battery electrode materials are crystalline, powder diffraction can provide time-resolved information on the evolution of the phase composition (e.g. formation of solid solutions and phase transitions), the average crystal structures (variations in the cell parameters, (de-)inserted ion localization in the crystal structure and site occupancy) and the microstructure (micro-strains and coherent diffraction domain size) occurring during the redox reactions involved in battery operation. The emergence of synchrotron and dedicated instrumentation (optics and experimental station) expanded the range of operation by increasing the flux on the sample, contributing to a better signal-to-noise ratio and also enabling a much faster acquisition time. The former allows spotting of weak peaks, which can enable the detection of otherwise elusive phases induced by ion ordering29,30 or the formation of incommensurate structures.31 Faster acquisition opens the possibility to perform experiments at much higher rates such as 60C (ref. 32) but more importantly, it pushed towards the development of high throughput setups for serial data acquisition on several batteries operating in parallel.17,33 Indeed, intermittent sample probing enables following several cells simultaneously (which usually offers enough data points, unless the aim is to follow short-lived intermediates), while at the same time reducing beam exposure and hence minimizing potential beam damage. In addition to that, fast data collection can be used as a mesh mapping tool in a single cell for tracking inhomogeneities (see below).
Better energy and angular resolution should enable a more accurate refinement of the crystal structures of the phases observed from the data collected operando.33 In addition, energy tunability enables optimizing the powder diffraction conditions (operate in transmission and minimize absorption by the cell casing), while also offering the possibility to couple powder diffraction and hard X-ray absorption techniques.34
The emergence of high energetic and high brilliance 3rd generation synchrotron sources, together with improved optics (Kirkpatrick–Baez mirror setups and refractive lenses), has made possible to standardly decrease beam sizes, in the micrometer range first, and ultimately down to the diffraction limit in the very hard regime (<20 nm at ∼100 keV). These conditions open the way to operando XRD microdiffraction, which was typically used to study the phase evolution of individual LiFePO4 nanoparticles and provided fundamental insights into the rate dependence of the redox mechanism for this compound, widely used in commercial cells.35 In this case, the small beam illuminated a finite number of grains whose Bragg reflection spots could be discriminated. This approach has recently enabled following the lithium concentration across a 80 μm thick graphite electrode, detecting and quantifying heterogeneities.36 One step further consists in probing a single particle using XRD-tomography based techniques allowing the visualization of cracks and strains in LiNi0.8Mn0.1Co0.1O2 induced during battery operation and contributing to capacity fading.37
Most often experiments in a synchrotron are carried out in transmission mode, with the incident beam along the electrode stacking direction. While this enables simpler alignment of the cell, it prevents the detection of inhomogeneities, which can arise in thick electrodes and are relevant in commercial batteries, especially at high operation rates. A possible alternative is to direct the beam parallel to the battery layers, in grazing incident geometry.38 This geometry enables tuning energy and/or changing the incident angle and can be useful for depth profiling experiments. This can be extremely useful to get a better understanding on how electrochemical reactions propagate but additional considerations apply as misalignment effects can easily interfere with the interpretation of results. Probing the electrode material at different cell locations and depth profiling are also possible using a pencil size beam coupled to energy dispersive diffraction.39,40 In this case, specific detectors able to discriminate energy are required and data treatment is also somewhat more complex but the advantage is that the probed volume, defined by incoming and scattered beams, remains constant, which is particularly valuable when dealing with very small beams.
The maturity of the operando X-ray diffraction approach does also manifest in the development of multimodal approaches coupling it to other complementary techniques (often also operando and hence using cell setups compatible with both). A meaningful illustration of this methodology is the combination of energy dispersive diffraction and X-ray tomography, which have enabled the visualization of the degradation of the InLi alloy electrode/Li10SnP2S12 electrolyte interface in all solid-state cells41 and to get further insights into the mechanism of anion intercalation in aluminium cells using graphite positive electrodes.42
With the improvement of synchrotron facilities, experiments at high energy (∼80 keV) have enabled penetration depths on the order of 1 mm with very good spatial resolution (ultimately related to focusing optics). One of its main advantages is the possibility to use real commercial cells in the experiments, such as pouch LiNixMnyCo1−x−yO2/hard carbon44 or 18650 LiFePO4/graphite for which phase transitions at both electrodes could be followed at a relatively fast rate (4C).45 In the former case, the lattice expansion of the Cu current collector enabled measuring the temperature and probing different regions of the cell allowed the drawing of 2D maps, which despite limited spatial resolution (0.3 mm, beam size) facilitated the detection of inhomogeneities (see Fig. 3). Last but not least, it is also worth mentioning that recent operando studies under optimized conditions at 107.7 keV (0.1173 Å) have permitted to follow the homogeneity of the lithium plating/stripping process in an “anode-free” pouch cell despite the low scattering factor of lithium.46
Fig. 3 (a) Experimental setup for in situ grid mapping (white dots) and operando position tracking (red diamonds: P1, P2, and P3) for graphite/LiNi0.5Mn0.3Co0.2O2 (NMC532) single layer pouch cells. (b) Contour plot for NMC532 and LixC6 reflections of interest collected at P3 during charge and discharge. (c) Diffraction line scan across the pressure interface (black dotted line in (a)). (d) The evolution of voltage during the 10th cycle together with selected NMC peaks and cell volumes, with marker sizes indicating phase fractions. Reproduced from ref. 43 with permission, © Elsevier. |
In order to achieve data over a relevant range of momentum transfer (Q) to reach low r values, high energies (>45 keV) and large angular coverage of the detector are required, which are only available in some specific beamlines. Otherwise, the situation would be similar to laboratory X-ray sources for which the energy is limited (maximum 25 keV with an Ag source) and the flux much lower. Nonetheless, despite these issues, Pair Distribution Function analysis is being increasingly used.47 Its result is a histogram of pair distances in the real space, but Fourier transformation is required due to data being collected in the reciprocal space. Operando total scattering experiments are challenging because a low, constant and reproducible background is required to extract reliable data, and this makes the cell design much more critical than for diffraction, which focuses on sharper Bragg peaks.48
This technique does also place additional requirements on the cells to be employed. If using high energy radiation and a small sample to 2D detector distance (typically 100 mm), flat cells will result in different absorption at high angles and thus a cylindrical geometry is more suitable. In addition to that, a blank cell needs to be measured to remove its contribution. Data treatment can also be complex. The small box modelling approach requires the crystal structure as an input and then the B (Debye–Waller) factors or selected atom positions can be refined. Discrepancy in PDF calculated values with respect to the average crystal structure can be attributed to local effects such as slight variations of bond distances. Another possibility is big box modelling including all atoms in a given volume and adjusting their positions to match the experimental data. Yet, this is only viable for small nanosized particles with a limited number of atoms and involves a significant computing time.
Overall, besides the limitations explained above, the experimental setup is not significantly different from that of conventional powder diffraction, and both depth profiling or combination with other techniques (e.g. tomography)49 are also possible. Nonetheless operando PDF insights are especially valuable for materials with a disordered crystal structure for which diffraction cannot provide information. Besides innovative materials, such as transition metal oxides with a disordered rock salt type structure used as positive electrodes in lithium ion cells,48 one particularly interesting case is non-graphitizable hard carbon, which has a structure consisting of graphene nanosheets with significant turbostratic disorder. Hard carbon is the negative electrode material of choice in sodium-ion batteries, a technology being already in the manufacture phase by several start-up companies and subject of intensive study. In this case, despite the difficulties in finding a suitable structural model and the overlaps from scattering by the electrolyte,50 meaningful data could be achieved which enabled to correlate pyrolysis temperature with the presence local structural defects and the electrochemical performance while also shedding light on the currently controversial redox mechanism.
This technique has been useful in probing reaction mechanisms both in materials which are already at the commercialization scale (or close to) for the Li-ion technology (e.g. silicon–graphite based composites as negative electrodes)52,53 and also in the mechanistic study of alternative chemistries such as the Li–O2 concept.54 In the former case, monitoring the silicon particle active volume by SAXS concomitant with the stage formation in graphite inferred from WAXS enabled the degree of lithiation in each component (affected by the cycling rate) to be independently followed, and also the assessment of the effect of pre-lithiation. In the latter, the growth mechanism of Li2O2 upon oxygen reduction in weakly solvating electrolytes is investigated, with results seemingly dismissing previous beliefs about the formation of a passivating conformal Li2O2 film which would intrinsically limit the achievable electrochemical capacity.
A great advantage of XAS is that it is element specific and probes short-range order, giving structural and chemical information of not only crystalline samples but also amorphous materials, liquids, gases, and complexes in solution, including highly diluted systems. The X-ray absorption near-edge structure (XANES) range of the spectrum corresponds to the electronic configuration and it is sensitive to the oxidation state of the element. Moreover, as the excitation energy is just sufficient to allow the photo-ejected core electron to reach the continuum, the photo-ejected electron wavelength is relatively large with respect to the interatomic distances, and the global XANES shape can be used as a fingerprint of chemical species. Instead, the EXAFS region of the spectrum corresponds to photo-ejected core-electrons of relatively high energy, with wavelengths comparable to the interatomic distances. In this region, the EXAFS oscillations can be modelled in the single scattering approximation obtaining quantitative information on the interatomic distances, kind and number of atoms surrounding the absorber and their relative disorder. Typically, EXAFS studies are performed at room temperature, for example as a function of state-of-charge, to access information on the charge compensation mechanism. Interesting complementary information can be achieved by ex situ temperature dependent EXAFS studies. Such measurements allow the local bond strength and structural disorder to be quantitatively accessed, both parameters affecting the final electrochemical properties. In particular, the local bond strength depends on the absorber-ligand orbital overlap, which affects the redox process. In this sense, it has been recently proposed that a larger degree of overlap between the transition metal and oxygen electronic states in Li-rich NMC increases the rigidity of the oxygen sublattice upon lithium deintercalation and results in a more reversible oxygen redox.57,58 Following the evolution of the EXAFS oscillations as a function of the temperature enables the experimental elucidation of changes in the local structure resulting from the redox process. Moreover, low temperature EXAFS data allow the quantification of the static disorder, which affects the diffusion coefficients of the intercalating ions. For instance, both local static disorder and bond strength have been found to influence capacity in NaxCoO2.59
Whenever possible, XAS spectra are recorded in transmission to achieve a higher signal-to-noise ratio. This allows for a fast scanning speed and is bulk sensitive, as the beam crosses the full sample or cell. In contrast, fluorescence acquisition mode shows typically lower signal-to-noise ratios and requires slower scanning speeds. It is used to investigate non-X-ray transparent samples or highly diluted systems.60 Alternatively or complementarily, XAS measurements in total electron yield (TEY) mode benefit from a high signal-to-noise ratio, fast scanning speed and surface sensitivity. The fundamental principles of the XAS method and progress of the instrumentation as well as the data analysis of both XANES and EXAFS have been covered in detail in several recent reviews such as ref. 61 and 62.
Experimental advances and improvements of synchrotron radiation sources lead to the development of Quick scanning EXAFS (QEXAFS), which pushed the acquisition time of a single spectrum in real-time from tens of minutes down to the sub-second regime. It has become an ideal tool for operando investigations of the kinetics of electrochemical reactions in batteries.77 The sub-second QEXAFS technique is based on specialized X-ray monochromators, which enable rapid and continuous energy scans by smoothly oscillating the monochromator crystals.78,79 The achievable temporal resolution is limited by the mechanical stability of the monochromator, the response times of the detectors, and the available photon flux. QEXAFS has been employed to study nonequilibrium phase transitions in LiNi0.33Mn0.33Co0.33O2 at high rates, enabling to determine that the redox process on Ni ions occurs to a larger extent at higher C rates, which is consistent with the benefits in rate capability observed for high Ni content materials (Fig. 4a).75 XAS has also been used to investigate transition metal high-entropy oxides (HEOs), a class of conversion-type electrode materials studied for Li-ion batteries that integrate at least five elements into a single phase to increase the configurational entropy, which is expected to improve electrode reversibility and cycle life. The reaction products of these HEOs are nanometric, defective and poorly crystalline and thus difficult to probe via XRD. The complex charge storage mechanism of spinel type (CrMnFeNiCu)3O4 HEOs has been unveiled by operando quick XAS enabling to confirm that all five elements contribute to the charge capacity to different extents at each state of charge, the processes being in some cases non- or poorly reversible, especially the reoxidation of Cu0 to Cu2+ (Fig. 4b).76
Fig. 4 Two examples of operando quick-scanning XAS: (a) XANES results of LiNi0.33Mn0.33Co0.33O2 at Ni, Co, and Mn K-edges throughout oxidation at a 30C rate. Ni K-edge energy shifts as a function of nominal lithium content x in NMC during oxidation at different rates (1C, 10C, and 30C). Reproduced from ref. 75 with permission ©John Wiley&Sons. (b) Voltage vs. capacity profile for the (CrMnFeNiCu)3O4 HEO electrode, and corresponding XAS spectra which enable changes in the oxidation state/coordination for the involved metal ions to be inferred as a function of the electrode state of charge.76 |
Fig. 5 (a) Illustration of a novel approach to investigate the SEI on silicon thin-film electrodes in situ through transmission sXAS and (b) extraction of the SEI spectrum from the overshadowing electrolyte spectrum and subtraction of the bubble and beam damage.82 |
The tender X-ray (TX) range, in which the K-edges of several relevant elements used in batteries, such as Na, Mg, Al, Si, and P, are located is unfortunately not commonly accessible. Indeed, it is often too high for sXAS beamlines and too low for most hard X-ray XAS beamlines. However, the penetration depths are longer that those of soft X-rays, so that conventional coin cells can be employed for operando measurements provided that the window is thin and composed of light elements, with Be, Si3N4 or Kapton being the most commonly used. On the other hand, the attenuation length is too low to measure in transmission mode and therefore FY is preferred.
Operando XAS on Li/S or Na/S batteries19,85,86 has shed light on sulfur speciation during the redox process and on the mechanisms that govern dissolution and deposition processes (Fig. 6). The different polyanionic species formed during cell operation are easily distinguishable by linear combination fits (LCFs) as their absorption edges. Spatially resolved XAS has been used to differentiate between the intermediate species present in the positive electrode and the separator of an operating Li/S cell during the first and second cycles87 and time-resolved operando XAS experiments with sub-second time resolution provided insights into the effect of the discharge rate in the redox mechanism.88 Finally, it is also worth mentioning that P K-edge XAS on LiFePO4 electrodes could also be followed via operando TX-XAS.89
Fig. 6 (a) Scheme of coin cells allowing measuring S K-edge operando in fluorescence mode. (b) Sulfur K-edge XANES evolution as a function of the state of charge followed operando in Na/S batteries and (c) selected spectra at various states during the first cycle with positions for reference compounds highlighted by vertical dotted lines. Reproduced from ref. 19, © John Wiley&Sons. |
In addition to the absorption techniques mentioned above which are based on electronic transitions to unoccupied states, X-ray emission spectroscopy (XES) is especially suited to probe the occupied states, including the valence electrons. Probing emission lines one can infer not only on the emitter's oxidation and local spin state, but also on the ligand nature. Studies combining XES and XAS revealed that Mn3+/Mn4+ play an active counterbalancing role during oxygen redox reactions in lithium- and manganese-rich layered oxides.90Operando XAS enables also multi-technique approaches combining XANES and EXAFS with sXAS, XES, and even other inelastic scattering techniques, such as resonant inelastic X-ray scattering (RIXS) or X-ray Raman scattering (XRS), the latter giving access to soft X-ray absorption edges by exploiting hard X-rays, i.e. with bulk sensitivity.74 Complementary studies involving sXAS and RIXS were especially useful to probe light elements such as oxygen. This enabled the correlation of the mechanism of generation of O2− and dimerization to form (O2)n− with the localization of electrons–holes primarily on the oxygen atoms in Li1.2Ni0.13Co0.13Mn0.54O2. By investigating the local environment around the transition metal ions using XANES it was evidenced that Mn4+ plays a specific role in trapping the holes on the oxygen atoms that ultimately determine the fine balance between oxygen loss and reversible oxygen redox in the operation of these electrode materials.66
hν − Ekin = Efin − Ein = BE + Φ | (1) |
Since the right part of eqn (1) is determined by the material, the actual Ekin range is controlled by the chosen hν photon energy. While electrons interact with any atom following a universal curve,94,95 the penetration depth of X-rays strongly depends on the elements they interact with, in particular when they are specifically absorbed to excite transitions. Nonetheless, the electron inelastic free mean path tends to be much shorter than the penetration depth of X-rays of the same energy (1 nm at 500 eV and 10 nm at 10 keV). Even in gaseous phases, the free path is short, and therefore for sufficient electron collection either ultra-high vacuum (UHV) or short paths at higher pressure are necessary. The availability at synchrotrons of hard X-ray photoelectron spectroscopy (HAXPES) has significantly expanded the sampling depth, overcoming some of the important limitations of lab-scale XPS. In fact, the high surface sensitivity makes challenging even ex situ characterization. Surfaces are easily affected by interaction with the atmosphere and adsorbates or reacted surface layers need to be removed after introducing the sample in a vacuum by either heating or gas sputtering with an ion gun. Even when applied carefully, such methods will hardly leave an exact representation of a fresh surface of the electrode material that may be of interest. For the same risk of altering composition and redox states, caution must be used in depth profiling studies assisted by sputtering.96 The non-destructive depth profiling offered by varying the photon energy with a synchrotron source is particularly attractive, as the electrode surface is often the subject of interest (investigation of passivation and SEI layers, which may exhibit a complex composite gel-like structure). In these cases, manipulation may still largely affect surfaces, and ensuring representativity is not straightforward. To exclude the impact of environmental contamination, the integration of chambers enabling to perform electrochemical experiments and handle samples directly connected to the analyzer chamber has been proposed.97 However, introducing surfaces wet with complex organic/inorganic mixtures directly into a vacuum poses a problem to the SEI integrity. Near ambient pressure photoelectron spectroscopy (NAPP) has mitigated this problem. By differential pumping, it is possible to keep a higher pressure close to the sample surface, so that fast drying is avoided, and the liquid electrolyte can be measured during hours simultaneously to the solid electrode.98 Other approaches for SEI analysis have addressed the formation of electrochemical interfaces by in situ (UHV) step-by-step deposition of solid electrolytes on top of electrode materials, which allows the study of dipole formations by following the shifts of the characteristic peaks of the substrate and electrolyte.99Operando XPS experiments would eliminate the effects of variable ambient contamination, but are more difficult to envisage. To observe effects comparable to the application of a bias, the charging produced by irradiation of an electron gun has been exploited to generate a so-called “virtual electrode”100 and explore interactions between metallic lithium and sulfide solid electrolytes. The most straightforward option for truly operando photoemission measurements is using solid state cells. One early example was based on a Na β′′-alumina plate to study the electronic effects of Na intercalation on a top layer of in situ prepared TiS2.101 More recent work studied the reactivity to oxygen of RGO deposited onto a solid glass-ceramic NASICON-type electrolyte in an ambient pressure XPS chamber. The resulting solid-state Li/O2 battery positive electrode demonstrated the intrinsic instability of most carbon defects to the oxygen radicals.102 Some operando studies with laboratory XPS could reveal chemical and electrochemical degradation at the interface between the two components of the electrode and sulfide solid electrolyte.103–105 The method is based on the observation of an electrode fabricated as a composite between the electrode active material and the solid electrolyte, so that both components and their interface are observed simultaneously. However, with the availability of HAXPES, it is now possible to study full solid state batteries. With a 10 nm Al collector on top of a 35 nm LiCoO2 layer, the P 1s signal of the garnet solid state electrolyte beneath the positive electrode could be observed, in addition to the signal of the remaining elements Al, Li, Co, and O.106 With liquid electrolytes, the feasibility of cells containing ionic liquids has been demonstrated in UHV.107 Instead, the use of more conventional organic or aqueous electrolytes is still limited, although technical advances have been possible with the introduction of graphene windows for the observation of liquids108 and the availability of liquid flow cells supporting graphene or Si3N4 windows that with a typical thickness of 25–50 nm can be crossed by electrons emitted from harder X-rays.109 Such experiments are becoming frequent especially in catalysis.110 Another approach for liquid electrolytes, requiring NAPP, is the “meniscus XPS” or “dip and pull” method.111 It consists in pulling the electrode out of the electrolyte so that it forms a nm-thick layer. These configurations are depicted in Fig. 7. Examples of experiments involving liquid electrolytes are still scarce, mainly because of the limited availability of beamlines capable of HAXPES and near ambient conditions. One example is the HIPPIE beamline at the MAX IV laboratory that is designed for in situ and operando NAPP experiments at the solid–liquid (dip-and-pull setup) interfaces under full electrochemical control.112,113 In addition, the radiolysis problems, discussed in the imaging section, represent a major challenge.114 As for other spectroscopic methods, the imaging mode has also been demonstrated operando, enabling for instance differentiation of lithium extraction rates from different facets of 10 μm LiCoO2 single particles, suggesting that the electrode rate capability can be improved by controlling the crystal habit.115
Fig. 7 Schematic representation of the original dip-and-pull method (a) and two variants (b and c) for XPS analysis of solid–liquid interfaces. Some of the electrons generated at the interface cross the liquid meniscus and are collected by the analyzer. Reproduced from ref. 116. |
Most of these studies are facilitated by tender and hard X-rays with higher penetration depths (several tens of nm), enabling operando experiments under more realistic conditions in terms of electrodes and electrolytes. On the other end, the use of soft X rays, even if increasing the surface sensitivity, allows much higher sensitivity to the lightest elements, including lithium, whose photoionization cross section is weak with laboratory radiation.
Despite that fact, coupling synchrotron radiation with FTIR microspectroscopy (SR-μFTIR) has great potential to study operando battery materials, as the synchrotron infrared source is 100–1000 times brighter than a conventional thermal (e.g. Globar) sources.120 Moreover, its high brightness (i.e. flux density) allows smaller regions (3–10 μm) to be probed in microscopy using different operation modes like transmission or reflection, suitable for operando battery analysis with an acceptable signal-to-noise ratio.121
In addition to the brightness advantage, the synchrotron source has other unique features. For example, the broad band of the synchrotron light enables FTIR spectroscopy to exploit the full infrared spectrum expanding from the far- to near-infrared regions of the electromagnetic spectrum. This is essential for determining the physical properties of solid-state components, to study surface science, as well as for the characterization of the chemical composition.122
Other advantages over the conventional thermal sources are a pulsed time structure and a high degree of polarization, which facilitate the combination of different techniques in a multimodal approach, especially when varying photon energies or frequencies are required. In this context, combining X-ray scattering, X-ray fluorescence (XRF) and X-ray absorption (XAS) with infrared microspectroscopic analysis on the same sample is of interest for a wide range of the materials research community. For instance, synchrotron infrared nanospectroscopy (SINS) combining synchrotron IR spectroscopy with scattering scanning near-field optical microscopy (s-SNOM) enables ultrabroadband infrared spectroscopy with nanometer spatial resolution beyond the Abbe limit (25 nm spatial resolution)123 and was used to investigate, in situ, the chemical composition of non-aqueous metal–air electrodes.124 For the sake of comparison, SR-μFTIR, with tens of micrometers field of view, allows a larger scale analysis area, while SINS enables estimating the chemical homogeneity at the nanodomain scale.
Despite the above-mentioned advantages, to the best of our knowledge there is currently no report on operando battery μFTIR measurement using synchrotron radiation. This can be rationalized considering the significant challenges associated with the development of a suitable electrochemical cell. Indeed, in situ/operando experiments using the attenuated total reflectance ATR-FTIR technique require the presence of an IR crystal of high refractive index (i.e. Ge, ZnSe, and diamond) and an IR transparent window (Fig. 8). The latter should be thin enough to allow for the required frequency range of the incident light to reach the sample and be reflected back to the detector. In addition to that, the presence of a thin layer of the electrolyte in the optical pathway can also represent a great challenge in terms of data treatment as the signal related to the electrolyte could mask the one originating from the system to be investigated.
Fig. 8 Schematic representation of the ATR-IR pouch cell on a Ge ATR crystal. Reproduced from ref. 119. |
Another important parameter to account for in ATR-FTIR measurement mode is the probing depth (dp), typically ranging between a few hundreds of nm and 10–15 μm.119
(2) |
with (λ) the wavelength of the light, (θ) the angle of incidence, and (n1) and (n2) the refraction indices of the IR transparent window and the probed medium, respectively (Fig. 7). Therefore, a higher penetration depth can be achieved using a low refractive index transparent window and measuring in the low frequency region. However, most of the signal is associated with the small fraction of the electrode/electrolyte (<ca. 15 μm) portion in direct contact with the transparent window. In order to minimize the contribution from the bulk electrolyte, FTIR difference spectra can be obtained by subtracting the initial spectrum before the start of the electrochemical characterization from each of the obtained IR spectra during cell operation.119
Most operando IR battery measurements were performed using (ATR-FTIR) spectroscopy coupled to conventional thermal sources in the mid-IR spectral range where high (spatial and temporal) resolutions are not required for which SR should not provide significant improvement in terms of data quality or spectral resolution. Overall, the main advantage of SR over conventional in-house sources is thus expected to be mostly related to far-FTIR spectroscopy and FTIR microspectroscopy, which is yet a challenging approach.
Far-IR spectroscopy (terahertz region) is a robust tool to probe many of the fundamental spectral features of the inorganic materials used in batteries since they exhibit a considerable number of rotational modes and characteristic vibrations in the low-wavenumber region of the IR spectrum. Yet, synchrotron far-IR spectroscopy operando or ex situ studies on battery materials have not been reported to date.
Most of the reported ATR-FTIR in situ/operando studies on battery materials focus on single point measurements (around 100 μm of diameter) obtained through co-added scans FTIR spectra during cell operation. This approach can however be misguiding as it is complicated to know if the point sampled is representative of the entire electrode. Therefore, it is necessary to perform multiple/raster scan measurements to verify the chemical composition along the electrodes and the data collected can be used to visualize chemical differences across the sample.125 Each pixel in a FTIR image is a complete infrared spectrum and hence by generating a sequence of FTIR images, it is conceivable to track variations in both space and time. Since the IR intensity of conventional sources is normally weak at high spatial resolutions (3–10 μm), especially when used in reflection (surface characterization), it requires a relatively long time (several minutes) to produce spectra with an acceptable signal-to-noise ratio at each measurement point and raster scanning experiments can be quite time consuming. The use of synchrotron-based FTIR imaging is thus a very promising alternative allowing hundreds of measurements to be rapidly performed over a large area of the electrodes with improved spatial resolution and serves as well to detect heterogeneities.
Fig. 9 Schematic representation of the four discussed techniques.127 (a) TXM, (b) STXM, (c) projection microscopy and (d) ptychography. In (a), (b) and (d) the numerical aperture (NA), i.e. the maximum angle at which the imaging system is able to collect photons from the sample is reported as a light red angle. The bigger is the NA, the larger will be the maximum collectable spatial frequency, and the smaller will be the spatial resolution in the image. In (c) the different imaging regimes in projection microscopy are given as a function of the ‘defocusing distance’ D = z1 × z2/(z1 + z2). Distances are not to scale. |
As schematized in Fig. 9a and b, for full-field and scanning modes the spatial resolution is limited by the lens numerical aperture (NA), i.e. the angular acceptance of the lens, to several X-ray wavelengths. In both cases, a spatial resolution down to 10 nm was demonstrated.128,129 In TXM (Fig. 9a), the sample is placed in the middle of two lenses, the condenser lens before the sample and the objective lens after the sample. The objective is the one that practically limits not only the spatial resolution but also the depth of focus of the imaging system.130,131 TXM is also compatible with Zernicke-type X-ray phase contrast.132 Phase contrast effects are intensity modulations due to the interference of beams caused by phase shifts that are induced by the interaction with a heterogeneous sample. In general, phase contrast techniques are particularly valuable when absorption is weak, as in the case of hard X-rays interaction with low absorbing (low Z) elements. In a STXM (Fig. 9b), a lens is placed before the sample, providing a well-focalized beam at the sample plane. The sample is then raster-scanned in the focalized beam, and the spot size will define the lateral resolution of the system.130,131 TXM is typically better in terms of the data acquisition speed with respect to STXM, which facilitates dynamic operando studies. The STXM setup is compatible with the acquisition of different types of signals (e.g., transmission, fluorescence, diffraction, TEY, etc.) which can be recorded simultaneously at each sample position. Among them, fluorescence detection results in elemental and chemical analysis with the best sensitivity and it is therefore often used as a complementary technique to simultaneous STXM.133 Another advantage of STXM is that since there are no lenses placed after the sample all the photons that reach it contribute to the image formation. This minimizes the necessary total dose delivered to the sample to achieve an acceptable signal-to-noise ratio and contrast, but not the resulting dose per unit time, which has to be always taken into account in the STXM scheme to consider possible beam damage of the sample.134 In projection microscopy (Fig. 9c), the image of the sample on the detector is obtained without the use of any lens, with the simplest experimental setup often also scaled down from the synchrotron to laboratory sources. In the particular case in which the detector is placed just after the sample, the setup is identical to standard radiography and the spatial resolution is directly determined by the detector pixel size. If instead the distance between the sample and the detector is large enough, the beam divergence can produce some magnification, and more importantly, also phase contrast effects.127 Among all the possible lens-less phase contrast techniques, the direct propagation-based phase contrast is the simplest experimental setup.135 The corresponding spatial resolution will depend on the used geometry136 and typically spans from several microns down to the sub-microns scale. For intermediate propagation distances (‘Fresnel region’ regime in Fig. 9c), the technique is usually called holography,137 whereas if the propagation distance is big enough (‘far field’ regime in Fig. 9c), widening the detected area well beyond the cone of beam illumination enables the so called ‘coherent scattering imaging’.135 In both cases, information on the sample structure and morphology can be deduced from the intensity distribution recorded on the detector via a ‘phase retrieval’ numerical reconstruction algorithm. Ptychography is the most frequent implementation of the coherent scattering- or diffraction-based imaging methods. In this case (see Fig. 8d), the object is illuminated by a coherent X-ray beam much smaller than the object size to image and the corresponding scattering pattern is recorded. Either the illumination or the sample is then shifted to a position with some overlap with the previous spot and the diffraction pattern recorded again. This process is repeated until the area of interest has been completely scanned. Because of the redundancy of information due to overlapping, phase retrieval algorithms converge quickly on a robust solution for both the object and the incident X-ray field. In this case, it is the detector geometry which limits the NA of the system, allowing for spatial resolutions down to a few nm (ref. 138) at the cost of the acquisition time. Interestingly, the ptychography setup is similar to the one used for STXM and both techniques may be implemented on the same instrument.139 The four techniques summarized in Fig. 9 can be used with either hard or soft X-rays and all allow tomographic 3D reconstructions if the cell can be rotated in an angular range big enough to collect enough information.140 When spatial resolutions below 100 nm are obtained in 3D by tomography, it is usual to refer to it as nano-tomography or, when it is implemented with the phase contrast approach, as phase-contrast nano-tomography.
Operando 3D tomography was first exploited with a cell that could be rotated 180°, on rather large SnO particles (10–30 μm) with a 2 μm resolution.145 In this case, an entire electrode, 16 mm diameter and 50 μm thick, was sampled, and typical crack evolution at the particle level was identified. In addition, different lithiation degrees in different electrode regions were inferred from the attenuation coefficient of absorption. First a Sn + Li2O composite was detected which was followed by an increase in Li-rich Li–Sn alloys, which are progressively less radiation absorbing because of the increased Li content. Absorption microtomography has become quite well established for operando studies in batteries, particularly for electrode materials containing heavy elements such as Sn and Ge, which provide the best contrast. Phase-contrast techniques are instead preferable for electrodes based on lighter elements. A 3D representation is particularly valuable in systems where the inherent reaction is a deposition process, such as the case of Li/S batteries, where degradation mechanisms can be sensitive to the morphological evolution of the deposits. The combination of absorption and phase contrast can be useful to discriminate different phases as shown in Fig. 10b. The sulfur particles, initially encapsulated by the binder to retain polysulfides, are progressively found distributed in the carbon electrode, while empty binder shells are left (Fig. 10d), which shows the failure of the encapsulation approach to prevent polysulfide dissolution.146 3D tomographic studies for this same battery technology have also revealed the coarsening of S particles in real carbon electrodes and depletion close to the separator147 resolving binder domains and electrolyte-filled bulk pores.141
Fig. 10 (a) 3D reconstruction of a pristine sulfur electrode showing non-woven carbon paper (NWC, dark grey) and Carbon-Binder Domains (CBD, light grey) coating the sulfur particles (yellow), with CBD partially removed to show sulfur; (b) comparison of absorption and phase contrast slices from the 3D segmentation; (c) combination of absorption and phase contrast segmentation (colours as in (a), except for sulfur, here in white). The star marks the same particle in the three images; (d) absorption X-ray image of the electrode after 2 cycles showing empty CBD shells (1) and white sulfur particles. In contact with the pore space (2) or with the conducting network (3). Reproduced from ref. 146. |
Si electrodes have been widely studied by phase-contrast tomography. Particle cracking, electrode volume, porosity evolution, and gas formation in the pores can be now quantified with a voxel size of 50 nm.148 These studies have been also combined with SXRD in the thickness of an electrode to track the presence of Li15Si4, which induces undesired volume expansion and strains/cracks in the electrode.149 Attempts have involved even metal-air batteries, where alkali oxides are particularly lightweight and with low absorption contrast with respect to carbon electrodes.150
Several operando studies have been reported for flow batteries, exploiting the difference in contrast between air and the electrolyte. The flow battery performance critically depends on the actual electrochemically active surface area and the electrolyte wetting of the carbon felt electrodes. Synchrotron X-ray tomography allowed the study of the effect of electrode compression on the electrolyte wetting of porous carbon electrodes.151 The flow distribution inside electrodes of different geometry was instead inferred by studying the flooding mechanism of the cell by the electrolyte at different flow speeds.152
These few examples illustrate that standard microtomography is useful to detect phenomena such as particle fragmentation or detachment enabling comprehensive sample statistics of geometric parameters. However, the picture may not be complete if resolution is not submicrometric, as the mechanical properties of smaller particles may significantly deviate from those of larger ones. Techniques able to attain nm resolution such as X-ray phase contrast nano-tomography seem a better compromise for submicrometric scale studies enabling statistics over several thousands of particle aggregates of a few μm, which can be considered representative of commercial battery electrodes. The detail of information makes possible sophisticated and precise parametrization of the particle geometry and arrangement, so that the particle architecture and electrode mesostructure can be optimized for electrochemical performance in a better way than with standard microtomography.153 However, in practice operando nanotomography has revealed quite challenging,153 mainly because of the small sampled volume, often below 50 μm in size, in comparison to the several hundred micrometers or mm typical for microtomography. This requires extremely precise cell assembly and alignment of the electrodes with cuts delimiting the studied region. However, their position can still be easily affected by expansion/contraction phenomena taking place during cell operation. Besides, even if employing high energy radiation that is weakly absorbed and generally considered non-invasive, the high intensity of the focused beam can cause interactions in the form of heating, binder disconnections, bubbles, and deviations from identical electrodes measured ex situ.150
Taking tomography images at different energies across an absorption edge in situ (i.e. pausing the electrical current during measurements) is considered to produce a so-called “5D” data set. Through a marker-less tomographic technique that simplifies sample preparation and automatizes alignment, 5D acquisition has been demonstrated by Wang et al.154 on a LiFePO4 electrode (Fig. 11) using a cell fitted inside a quartz capillary, to allow complete rotation. Characterization relied on a full-field hard X-ray TXM at the Fe K-edge deconvoluting spectra as combinations of LiFePO4 and FePO4 references with results indicating a biphasic mechanism with the absence of intermediate phases. Remarkably, this was only unambiguously inferred from 3D images, as 2D projection maps showed artefacts that might have been misinterpreted as intermediate phases present.
Fig. 11 Illustration of a 5D Fe K-edge XANES tomography. (a) Schematic of the experimental setup. A tomography data set is collected at different energies across the near Fe K-edge absorption to access chemical information for each voxel. By fitting the resulting spectra as a linear combination of spectra of end-phases, phase composition can be assigned to each voxel (right side). (b) Chemical phase distribution as a function of capacity (proportional to time). Reproduced from ref. 154. |
Miniaturized liquid cells allowing operando TEM have been developed in the past decade.156 Also several commercial systems are available, and their use with soft X-rays has been proposed (see for instance ref. 157). Typical cells adapted for soft X-rays operando imaging with liquid electrolytes consist of a flat transparent region, from a few hundreds of nanometres to ≈1 μm in thickness, confined between two ultrathin silicon nitride windows (typically <100 nm) and coupled with a microfluidic system with potential biasing158,159 (see Fig. 12 for a scheme). In the case of STXM in fluorescence mode, transmission is not required and hence the cell geometry can be simplified, with just one transparent window, and no submicrometric sample thickness.160 The construction of these miniaturized cells is in general significantly more challenging and expensive than the cells used in hard X-ray microscopy. Their representativity with respect to commercial batteries is hence limited and must be considered as setups for model experiments. Indeed, the thicknesses of the electrodes and electrolyte are so reduced that even the electrochemical processes may be affected. Although finite element calculations have shown that at the typical extremely low currents used the concentration and potential gradients in the electrolyte are negligible,158 the presence of flow and turbulences, the discrete deposited particles, and their contact with the current collector may all affect these miniaturized cells to a larger extent than macroscopic ones. There is certainly a need for understanding the details of the electrochemistry on such configurations, which might also be relevant for microbatteries. Also the radiochemistry of the irradiation at different soft X-ray energies on the most typical battery chemistries need an assessment. Indeed, a rich radical chemistry has been shown for electron irradiation on organic electrolytes of interest for lithium batteries.161 Complex radical cascades are induced by solvated electrons, involving solvent molecules and particularly salt anions. As a result, beam-induced electrochemistry can be observed, even in the absence of cell bias, sometimes preventing a reliable operando observation of electrode processes. For this reason, commercial TEM operando goniometers offer flow options for the electrolyte in a liquid cell, so that at least in situ observation can be interleaved with electrochemical operation, washing away the products of irradiation before electrochemistry is resumed. With X-ray radiation, although also significantly ionizing, a comparatively less dramatic radiolysis is expected, but this needs systematic assessment.
Fig. 12 Schematics of an electrochemical cell for operando TEM. The electrodes (WE: working; RE: reference; CE: counter) are connected to an external potentiostat. |
In spite of these constraints, some remarkable results have been achieved also with soft X-ray microscopy. The high spatial resolution was exploited in a detailed soft X-ray STXM study on 30 LiFePO4 particles of realistic size. It demonstrated slow and fast domains, and a different evolution upon oxidation and reduction.158 The biphasic behaviour was found to turn to a solid solution at a high rate with heterogeneities increasing/decreasing during delithiation and relithiation respectively. The observation of these phenomena provided key details in the understanding of the redox mechanism of this material, widely used in commercial batteries. Interestingly, a follow up study by soft X-ray ptychography157 enabled insights into the particle morphology (Fig. 13A–C) and chemical speciation thanks to the better spatial resolution (≈7 nm, still 4.3× the X-ray wavelength but 7× better than the STXM approach). Although qualitative agreement between the obtained chemical maps (Fig. 13D and E) is evident, the ptychographic one depicts nanoscale chemical phase features inside the particles, which are not visible with conventional STXM.
Fig. 13 Comparison between conventional STXM (A and B) and ptychographic (C and D) spectromicroscopy images of LixFePO4 microplatelets. The average optical density (A and C) and the chemical composition map (B and D) where the two chemical components (LiFePO4 and FePO4) are presented in green and red, respectively (scale bar is 1 μm; reconstructed pixel size 5 nm). (E) Point spectra from the dots marked in (B) by conventional STXM (dashed lines) and ptychographic modes (dotted lines with circles). Reference spectra from pure materials (LiFePO4, green solid line; FePO4, red solid line) are also shown for comparison. The conventional STXM spectra show distortions that flatten the sharpest peaks, corresponding to energies where the difference in absorption between phases is maximum. The different attenuation overweighs the more abundant phase and instead the ptychographic spectra more closely match the pure references. Reproduced from ref. 157. |
As a result of the cell setups being more straightforward when using solid electrolytes, the 3D morphological and chemical evolution of solid state batteries using X-ray tomography operando is quite established. Electrochemically driven phase changes, formation of cracks, contact loss and formation of interphases that increase electrode–electrolyte interface resistances have been visualized. For instance, the void formation at the interface between lithium and the Li10SnP2S12 solid electrolyte was identified by X-ray tomography as the primary cell failure cause.162 The chemomechanical interactions between the FeS2 conversion electrode material and a Li7P3S11 solid electrolyte were also studied by operando synchrotron X-ray nanotomography, which in this case enabled the detection of the loss of contact and build-up of metallic Fe which penalized Li diffusion, mitigated with a specially designed 3D electrode microstructure.163
All the above-mentioned techniques probe complementary aspects, while at the same time presenting different technical advantages and disadvantages, which have resulted in different maturity levels. To access which phases are composing the electrode materials and how they are evolving as a function of cycling, XRD, PDF and XAS are exploited. They probe the averaged and local structures with XRD accessing only crystalline phases and PDF and EXAFS needing a well-defined model for quantification, where different correlated parameters can bias interpretation. Microscopy may instead provide this information more immediately in a qualitative way but at a local scale, while FTIR and soft X-ray XAS provide precious information on the organic compounds at either the electrodes, electrolytes or interphases, which are typically not accessible by XRD, hard X-ray XAS, or PDF. XAS and XES can be exploited to assess charge compensation mechanisms being naturally complementary as they probe unoccupied and occupied electronic levels, respectively. Yet, since the spectral features depend on the electronic properties, site symmetry, and nature of bonding with surrounding ligands, their interpretation is not straightforward unless different edges are probed and/or different techniques are coupled.
One of the crucial aspects to assess is the improvement of cell design to be able to carry out operando experiments in setups which are representative of real battery operation. Indeed, while real pouch or even stainless steel casing coin or cylindrical cells can be used under very specific conditions, customized cells are the norm. Even if practical parameters such as the electrode formulation or the electrode/electrolyte amount ratio mimic realistic systems as much as possible, geometrical constrains may induce changes in the electric field lines which can have an influence on the electrochemical performance and hence also some impact on the phenomena investigated. As mentioned above, the complexity of the processes taking place during battery operation calls for the development of multi-modal characterization, i.e. the use of more than one technique in the same experiment (not necessarily both being synchrotron based), is a clear path to follow which enable achieving a more holistic understanding of the mechanisms involved. Ideally, it should involve the use of the same optimized cell setup and either correlative or even simultaneous standardized workflows, minimizing beam-induced effects, while at the same time adjusting the spectral response to the required time scale to follow cell dynamics. The development of an “ideal” cell representative of real batteries and suitable for any multimodal approach does not seem realistic, especially considering that the portfolio of techniques used is rapidly expanding, each of them coming with their own technical/geometrical requirements. However, as mentioned in the section devoted to electrochemical cells and setup requirements, progress in cell design has been outstanding in recent years, with some designs available (some being commercialized) that can already be used for a wide variety of techniques.
All operando synchrotron experiments are expected to allow non-invasive and non-destructive probing of materials under real conditions and hence enable even the detection of metastable intermediate species. However, ensuring that the beam has no effect on the investigated material is challenging. On one hand, exposure to high energy radiation can induce beam-induced effects and control experiments are mandatory to assess the reliability of data interpretation. If the beam induces some sort of irreversible damage (e.g. on the binder/carbon matrix),164 they will be more easily identified. Yet, effects can be more subtle and disappear when irradiation is stopped, which can make its detection more difficult, especially if new battery chemistries are investigated165 for which no standard components exist. These aspects become specially challenging for XAS and in particular for proper EXAFS measurements, as these require in general a relatively long exposition time at energies where intense absorption is present. Interaction with the beam is complex and can involve the emission of photoelectrons, Auger electron cascades, radiolysis phenomena, radical formation, electrolyte decomposition and gas bubble generation.5,165 Therefore, acquisition conditions need to be carefully optimized in each experiment to minimize beam induced effects. Typical strategies166 consist in defocusing the beam, reducing the local exposure time, performing stroboscopic measurements where acquisition is alternated with rest times, average measurements at different positions and attenuating the beam intensity. It will be critical to study and control all these phenomena in view of the ongoing shift to 4th generation synchrotron sources and free-electron lasers, which offer orders of magnitude higher photon intensities. These may open the possibility to greatly reduce exposure times but radiation damage induced by dose rate may still be a limiting factor. For such reasons we expect that when spectromicroscopy and tomography are used in the same experiment, it will remain practically unlikely to achieve true operando conditions due to the actual exposure times required. It will rather be preferable to stop the reaction and deal with in situ experiments, which generally do not imply the loss of reliability. For instance, comparable conclusions were drawn from ex situ soft X-ray TXM measurements167 and TEM operando168 studies on Na/O2 batteries, which can be considered a mutual validation for both techniques on this specific system. Overall, as in other research fields, common sense and a judicious choice of the methodology should prevail to make the most efficient use of available resources while maximizing scientific progress.
Another overriding and growing concern related to operando characterization is the huge amount of data produced, and the difficulties of their subsequent analysis. Different automated data treatment protocols have been recently developed such as the Pearson correlation coefficient, enabling to detect subtle changes in the materials present during high-throughput operando diffraction experiments,169,170 while also allowing to take decisions during data collection thanks to its mathematical simplicity. Other more mathematically complex methods, such as non-negative matrix factorization, have been developed to assist in elucidating the phases present/appearing in microscopy images or operando series.171,172 However, automated analysis able to obtain more physical information is only starting, e.g. following the profile changes of specific graphite diffraction peaks to infer the succession of stages formed during the redox process.173 The need to perform Rietveld refinements on a large number of successive XRD patterns has been addressed developing specific software enabling either automated fitting of single diffractograms (that can be expanded in a relatively simple way)174 or more complete tools specifically designed for sequential refinement of operando patterns.175 The complexity and instrument specificity of the data harvested using other techniques (and even also diffraction) clearly call for further developments in this area, with progress in big data and artificial intelligence being a clear asset. Besides data analysis, the automation of multi-technique data acquisition using standardized workflows would bring in a paradigm shift in operando characterization, especially if standardized cells could also be designed.3
Given the recent evolution achieved in these areas, accelerated progress is expected in the years to come which will certainly improve our ability to understand battery mechanisms at an atomic level and hence develop new chemistries while at the same time getting the most out of the already commercialized concepts.
This journal is © The Royal Society of Chemistry 2023 |