Graphene has attracted considerable attention due to its unique physical and chemical properties. Thanks to its atomic thickness, high carrier mobility, and transparency, graphene is the best electrode material for a wide range of optoelectronic devices such as solar cells, light-emitting diodes, and photodetectors. Improvement of graphene/silicon (Gr/Si) solar cells has gained significant research interest in the field of semiconductor devices. Herein, a comprehensive review of Gr/Si solar cells is provided with a detailed introduction of the structure, mechanism, and fundamental physics of Gr/Si solar cells. Then, various key strategies to improve the performance of the solar cells are summarized. The article concludes with the goals and direction for future works on graphene-based solar cells.
Conventional silicon solar cells based on p–n junctions have high efficiency and long-term stability,3 however, they have a high fabricating cost due to the need for high-quality silicon,and the complicated manufacturing steps restrict their widespread usage.4,5 New materials, technologies, and fabrication processes have, therefore, been explored. Solar cells with heterojunction structures, including carbon materials, have attracted much attention nowadays because carbon is a rich element in nature and can be made at low cost with economies of scale in production.6 Investigations of carbon materials have been carried out due to their structural variety and unique texture, features, and applications. Since the 1960s, new carbon materials that differ from traditional carbon materials (such as carbon black, activated carbon, and graphite) have been produced. Carbon nanomaterials, in the form of stable allotropes (such as carbon nanotubes, graphene, fullerene, nanofibers, etc.), are significant building blocks of nanotechnology.7 Notably, one-dimensional (1D) carbon nanotubes (CNTs) and two-dimensional (2D) graphene members of the family of carbon nanomaterials exhibit outstanding electronic and optoelectronic properties that make them excellent alternatives for energy conversion.8,9
Carbon nanotubes are hollow cylinders constructed by rolling up a graphene sheet, which is a vast planar hexagonal lattice of only sp2-bonded carbons first reported in 1991.10 Moreover, carbon nanotube has several benefits, including high charge carrier mobility, ballistic transport properties, high optical transmittance, and low light reflectance, which satisfies the prerequisite of heterojunction-based solar cells very well.11,12 However, there are challenges in setting up adequate contacts between CNTs and semiconducting materials, such as silicon, to create a working heterojunction.13 Graphene is another carbon nanomaterial, which has superior electrical, optical, and mechanical properties, high carrier mobility, as well as low absorbance,14–16 and can be manufactured and handled into ultrathin films,17,18 sheets,19–21 ribbons,22,23 fibers,24,25 and large-surface papers.26
Hence, the applications of this graphene have been widely investigated in different fields, from spectroscopy to nanoelectronic devices, photonics,27 solar cells,28–30 transistors,31 fuel cells,32,33 supercapacitors,34,35 photocatalysts,36 sensors,37 mass spectrometry,38 and drug delivery.39 In addition, with the introduction of graphene in 2004, many 2D materials were successfully manufactured using different methods, such as chemical and physical vapor deposition methods.40,41 Li et al. first demonstrated the synthesis of Gr by chemical vapor deposition, which is the standard and common technique to produce large-area and high-quality graphene sheets.42–44 In general, Graphene is an attractive material for optoelectronic devices due to its several merits over other materials.45–48
The flexibility of graphene can help to alter the crystal structure or size of carbon at the nano-scale and can greatly assist the investigators to adjust the electrical and optical features of carbon nanomaterial. Research has shown that carbon/silicon solar cells, which are formed by constructing a transparent carbon layer, especially in Si semiconductor silicon-based solar cells, indicate a good potential or prospect for the future of solar cells.47,48
Fig. 1 Chemical structure of graphene, graphene oxide (GO), and reduced graphene oxide (rGO). Reproduced from ref. 54, with permission from the Royal Society of Chemistry. |
Fig. 2 (a) Schematic of a graphene-on-semiconductor (Si) solar cell. (b) Electron–hole pairs transport across the surface junction. Reproduced from ref. 159, with permission from Elsevier. |
The mentioned parameters are the major criteria in the assessment of solar cell operation. All of them can be determined from the Current density–voltage curves of the devices exposed to solar simulator radiation under AM 1.5 conditions. When graphene/Si solar cells are open-circuited, the separation of photoelectric carriers generates Voc. When a solar cell is short-circuited, the separated photovoltaic carriers can pass over the external circuit, creating an Isc.
The current density (J) and open circuit voltage (Voc) of a silicon solar cell can be calculated by the following equations:63
J = Jsc − Js[exp(eV/ηkB − 1)] | (1) |
Voc = (ηkBT/e)ln[Jsc/Js + 1] | (2) |
The fill factor (FF) of a solar cell can be determined based on the ratio of maximum current density, Jmax, and voltage, Vmax to the product of Jsc and Voc.
The PCE of a solar cell is determined as the incident power converted into electricity which can be expressed by:64
FF = (JmaxVmax/JscVoc) | (3) |
PCE = (JscVocFF/Plight) × 100% | (4) |
For the sake of brevity, this short review avoids detailed descriptions of basic concepts which are illustrated in books on the topic of Gr/Si solar cells. In this sub-section, we examine the trend and enhancement of the main parameter in Gr/Si solar cells that were reported by some experimental results also can be categorized into three sectors:
1. Open circuit voltage improvement, which is associated with the height of the Schottky barrier.
2. Short circuit current density improvement, which is associated with the light absorption by silicon surface substrate.
3. Fill factor improvement, corresponds to the reduction of the minority carrier recombination.
This review concentrates only on the application of graphene in the structure of solar cell devices. Moreover, the band structure of graphene-based solar cells and alternative robust solutions for enhancing the performance of this kind of solar cell will be addressed. The limitations will be also discussed in the next sections.
On the other hand, the series resistance may be high for high sheet resistance. (2) The flat silicon wafer absorbs a limited number of photons (30–40% of visible light, 350–800 nm).67 Since the introduction of graphene/Si solar in 2010,68 various methods have been developed to adjust its work function, improve the conductivity of graphene, and reduce the reflectance of silicon wafers. These methods include chemical doping,69–74 increasing the number of the layers of graphene,75,76 and presenting an interlayer,77–82 controlling of the reflectivity with antireflection layer83 and using III–V semiconductors,84 all of which can optimize the efficiency of solar cells significantly.
The most suitable insulating layer materials for this purpose are silicon dioxide (SiO2),85,86 molybdenum disulfide (MoS2),87 aluminum oxide (Al2O3),88 graphene oxide (GO),89 hexagonal boron nitride (h-BN),90 poly(3-hexyl thiophene-2,5-diyl) (P3HT),91,92 quantum dots,93,94 Molybdenum trioxide (MoO3),95 and spiroOMeTAD.96
Song et al.97 used an optimal thickness of the SiO2 layer as a layered electron-blocking layered to improve the performance of the solar cell (Fig. 3(a)). Their outcomes indicated an increment in the efficiency of the device from 7.9% to 12.4% upon increasing the thickness of oxide from 5 to 15 Å (Fig. 3(b)). TiO2 anti-reflective coating (ARC) and chemical doping (AuCl3) were also employed in the solar cells with efficiencies as high as 15.6% (Fig. 3(c)).
Fig. 3 (a) Schematic representation of graphene/n-silicon solar cell. (b) J–V properties of graphene/n-silicon solar cell for various oxide thicknesses. (c) Comparison of two solar cells with and without oxide layer and anti-reflective coating (ARC). Reproduced from ref. 97, with permission from the American Chemical Society. (d) Schematic diagram of graphene/h-BN/Si device. (e) The band diagram of the graphene/Si solar cells with and without an h-BN layer. (f) J–V of the device with and without an interlayer. Reproduced from ref. 99, with permission from Elsevier. |
In another report, Jiao et al. and Yang et al.98 employed graphene oxide as an interfacial layer to improve the efficiency of the solar cell. They altered the annealing temperatures to achieve higher PCE values. By employing the GO film, the PCE declined from 2.13% to 0.2%, but after increasing the annealing temperature up to 400 °C, the efficiency showed an improvement of up to 5.2%. To reduce the surface recombination in the graphene/n-silicon solar cell, Meng et al.99 used a few-layer boron nitride (h-BN) which was sandwiched between graphene and n-silicon. It also offers the advantage of a hole transport layer. The few-layer graphene was synthesized on Cu foils by a low-pressure CVD method. As shown in Fig. 3(d), several layers of hBN and graphene were deposited onto a silicon substrate by the layer-by-layer (LBL) transfer process and the CVD method, respectively. Moreover, the band structure of the graphene/n-silicon solar cell is shown in Fig. 3(e) after modification. After depositing the hBN layer, photovoltaic properties such as Vocs and PCEs raised from 0.412 to 0.474 V and from 3.75% to 4.40% in the original cells, respectively (Fig. 3(f)). The graphene/h-BN/Si solar cell exhibited an initial PCE of 4.40%, which improved to 10.93% by co-doping of graphene with Au nanoparticles and HNO3. In contrast to SiO2 and Fluorograph, the hBN layer shows no trapped charge or surface states. Hexagonal Boron Nitride (hBN) is an sp2-hybridized 2D insulator with a very smooth surface having no dangling bonds. In addition, hBN is isoelectronic with a structure similar to graphene. Its low lattice mismatch (only 1.7%) allows compatible graphene/hBN heterostructures with suppressed interface recombination and elevated open-circuit voltage.100–103
Zhang et al.104 fabricated graphene nanowalls (GNWs)/Si solar cells and improved the device with an interface engineering solution. They also used a polymer-free transfer method (PFTM) of GNWs grown on the copper foil to manufacture the device. They fabricated three types of GNWs/Si solar cells to compare the effect of the spiro-OMeTAD interface layer. Fig. 4(a) demonstrates the diagram of three as-prepared solar cells, where A, B, and C illustrate spiro-OMeTAD/n-Si, GNWs/n-Si, and GNWs/spiro-OMeTAD/n-Si solar cells, respectively. It should be noted that spiroOMeTAD is a highly profitable p-type organic semiconductor with extensive applications as a hole-transport layer in organic devices (Fig. 4(b)). The Optimization of the thickness of the spiro-OMeTAD layer is also a significant parameter influencing the solar cell performance. Various thicknesses of the spiro-OMeTAD thin film were formed through diverse concentrations of the spin-coating solution (10–70 mg ml−1). The highest PCE (8.27%) was recorded in the case of the GNWs/spiro-OMeTAD/Si device, at the spiro-OMeTAD concentration of 30 mg ml−1 with an estimated layer thickness of ∼33 nm. Further increase in the concentration of the spiro-OMeTAD solution, however, led to the opposite effect (Fig. 4(c)). The effect of Molybdenum trioxide (MoO3) was investigated on the photovoltaic characteristics of graphene/Si solar cells by S. Chandramohan, et al.105 (Fig. 4(d)). MoO3 is one of the best transition metal oxides which can improve the work function of graphene. By employing the MoO3 onto graphene, the PCE was improved from 0.86% to 3.5% (Fig. 4(e)). A maximum efficiency of 4% was obtained for the MoO3/Ag/MoO3 multilayer (MAM) solar cell. The MoO3/Ag/MoO3/graphene structure showed a sheet resistance of 10 Ω sq−1, which is 98% and 97% lower than that of pristine graphene and MoO3-coated graphene, respectively.
Fig. 4 (a) Schematic structure of three sets of the devices: spiro-OMeTAD/n-Si solar cell; GNWs/n-Si solar cell; GNWs/spiro-OMeTAD/n-Si solar cell. (b) J–V characteristics of the three sets of structured GNWs/Si solar cells. (c) J–V characteristics of the device with different concentrations of the spiro-OMeTAD. Reproduced from ref. 104, with permission from American Institute of Physics. (d) Schematic diagram demonstrating the steps of device construction. (e) J–V characteristics of the devices manufactured with and without MoO3 film. Reproduced from ref. 105, with permission from Elsevier. |
In 2017, Alnuaimi et al.106 reported the improved performance of Gr/Si Schottky barrier solar cells (SBSC) by engineering the interface with the aluminum oxide (Al2O3) layer. The device structure and band diagram are shown in Fig. 5(a)–(c). The advantage of the Al2O3 interface layer is not just restricted to forming a higher Schottky barrier as it also decreases the recombination at the interface. In Schottky barrier solar cells (SBSC), the tunneling of holes should dominate over the recombination to gain effective charge carrier transport. Based on Song et al.107 the presence of a layer of native oxide at the interface between the graphene and silicon permits the tunneling of holes. But the native oxide thickness grows continually, declining the operation of Gr/Si solar cells over time. As displayed in Fig. 5(b), by increasing the native oxide thickness, the tunneling of holes decreases. This phenomenon leads to accumulation at the interface, increasing the charge carrier recombination. Therefore, the use of the SiO2 intermediate layer poses a major problem affecting the performance stability of Gr/Si SBSC. As indicated in Fig. 5(c), deposition of the Al2O3 layer on the native oxide surface controls the creation of thick native oxide at the interface. The formation of the Al2O3 layer also helps in decreasing surface recombination, enhancing the carrier lifetime for the silicon surface, and declining the series resistance. Thus, the enhancement in solar cell efficiency with the Al2O3 interfacial layer can be assigned to the passivation of the silicon surface, which diminishes surface recombination, leading to higher SBH, which facilitates the transport of charge carriers. Al2O3-containing solar cells indicated an enhancement in PCE from 7.2% to 8.7% and acceptable stability after 28 days of operation (Fig. 5(d) and (e)).
Fig. 5 (a) Schematic of Gr/Al2O3/Si device. (b) and (c) the energy band diagram of devices with and without Al2O3 layer. (d) J–V characteristics of devices. (e) Variations of PCE and Voc of Gr/Si with Al2O3 interfacial layer by time. Reproduced from ref. 106, with permission from the Royal Society of Chemistry. (f) Metal–insulator–semiconductor Schottky solar cells by Al2O3 layer. (g) J–V characteristics of the devices under illumination with and without an Al2O3 layer. (h) Comparison of J–V for different thicknesses of the Al2O3 layer. Reproduced from ref. 108, with permission from Elsevier. |
In another study, Rehman et al.108 manufactured a high-efficiency n-type textured Si/Al2O3 solar cell by instant transfer of graphene on the substrate using plasma enhanced chemical vapor deposition (PECVD) (Fig. 5(f)). They transfer a small number of layers of graphene on top of Al2O3/Si through plasma-enhanced chemical vapor deposition. Finally, by optimizing the thickness of the Al2O3 layer interlayer (30 Å), the maximum efficiency of 8.4% was obtained without passivation thin film or intentional doping due to decreased surface recombination at the interface (Fig. 5(g) and (h)).
MoS2 layers in graphene solar cells have attracted great attention in recent years due to their unique band structure, high absorption coefficient, and electrical properties. The MoS2 interlayer can operate as a hole transport layer to simplify the separation of electron–hole pairs. Moreover, it acts as an electron blocking layer to quench the recombination at the interface. Ma et al.109 prepared a high-efficiency graphene/MoS2/Si solar cell (Fig. 6(a)) in which the graphene and MoS2 monolayers were deposited by a spin-coated method. The MoS2 interlayers could dramatically enhance the efficiency of the device and the thickness of the layer could be controlled via direct sulfurization of pre-annealed molybdenum foil. By optimizing the thickness of MoS2 layers (4 nm), a high efficiency (13.1%) was achieved for graphene/MoS2/Si Schottky barrier solar cells (Fig. 6(b)). Likewise, TiO2 anti-reflective coating (ARC) was also used which incremented the efficiency to 15.8% (Fig. 6(c)).
Fig. 6 (a) A schematic representation of graphene/MoS2/Si Schottky barrier solar cells. (b) J–V characteristic of graphene/MoS2/Si Schottky solar cells. (c) J–V characteristics of the device with antireflective layer. Reproduced from ref. 109, with permission from Elsevier. (d) Schematic design of metal–insulator–semiconductor with GOQD interlayer barrier. (e and f) J–V characteristic curve for the optimal GOQD size and thickness. Reproduced from ref. 110, with permission from Science Partner Journals. (g) Schematic structure of the Gr/CQDs/Si solar cells. (h) J–V characteristics of the Gr/CQDs/Si solar cells. Reproduced from ref. 111, with permission from Science Partner Journals. (i) J–V characteristic of the solar cells with/without GQDs. Reproduced from ref. 112, with permission from Elsevier. |
The effect of the graphene oxide quantum dots (GOQDs), as a high-quality interfacial, were explored layer on the graphene/n-Si solar cells by Geng et al.110 GOQDs can adjust the interface properties of Gr/Si Schottky barrier solar cells (SBSCs) and act as a distinctive barrier at the interface (Fig. 6(d)). The association between PCE and the particle size and thickness of GOQDs was also evaluated. The hole tunneling and the carrier recombination rate can be handled by the thickness and particle size of the GOQDs barrier in the Gr/Si SBSCs. The GOQD-induced additional band flexure in Gr/Si-based SBSCs supplies a process for enhanced PCE. The best efficiency (with Jsc, Voc, FF, and PCE of 19.01 mA cm−2, 0.47 V, 74.07, and 6.75) was recorded at the GOQDs size of 4.15 (Fig. 6(e)). The optimal GOQD thickness was 26 nm as Jsat of the solar cell drops from 2.19 × 10−8 A cm−2 to 8.14 × 10−9 A cm−2, suggesting that the carrier recombination is virtually stifled. According to their result, the best PCE of Gr/Si-based SBSC (6.75%) was recorded at the optimal particle size and thickness of 4.15 nm and 26 nm, respectively (Fig. 6(f)). After employing the TiO2 nanoparticles and doping HNO3, the PCE efficiency rose to 13.67%. Geng et al.111 reported high-efficiency Gr/Si solar cells by using carbon quantum dots (CQDs) as interfacial modification layer (Fig. 6(g)). The CQDs interlayer was used as both an electron blocking and hole transport film, showing a more inferior reverse saturation current and more considerable Voc which enhances the solar cell performance. The PCE of resulting Gr/CQDs/Si solar cells is 6.52%. The optimal PCE was achieved by fine-adjusting the thickness and sizes of CQDs interlayer to 26 nm and 4–7 nm, respectively without chemical doping. Their result showed that the PCE of 9.97% upon using the nano-TiO2 (Fig. 6(h)).
Jang, Chan Wook et al.112 manufactured a highly efficient GR (TFSA-GR) TCE/GQDs/PSi/n-Si/BCP solar cell. The graphene quantum dots (GQDs) serve as an interfacial layer for proper band alignment between GR transparent conductive electrode (TCE) and silicon as well as reducing the electron–hole recombination at the junction interface, hence, improving the PCE performance. Similarly, the lifetime of the hot carriers in GQDs is fairly long which is beneficial for the efficient harvesting of hot carriers and carrier generation. Moreover, they employed Bathocuproine (BCP) as passivating layers to block the carrier recombination at the Si back surface. The mentioned two approaches declined the carrier recombination at the GR TCE/PSi and Si/cathode interfaces, respectively. An enhancement was observed in the PCE of TFSA-GR/GQDs/PSi/n-Si solar cell (13.66%) upon BCP as compared to the original solar cell (12.35%) (Fig. 6(i)).
Diao et al.113 manufactured highly efficient GQDs/n-silicon heterojunction solar cells (Fig. 7(a)). They employed the GQDs layer due to their unique electrical transfer characteristics and band structures which can serve as an electron blocking layer to stifle the carrier recombination at the anode. They prepared GQDs of different sizes and thicknesses by altering some synthesis parameters. Fig. 7(b)–(h) illustrates the current density–voltage curves and EQE of the GQDs/Si heterojunction solar cells with various sizes and thicknesses of the GQDs. Atomic force microscope (AFM) images in Fig. 7(d)–(f) shows the extreme roughness of the GQDs layers on the substrates due to the aggregation of GQDs, hindering the determination of the layer thickness. Nevertheless, an average of 8, 20, and 50 nm were calculated from the AFM images. The solar cell efficiency was under the influence of the sizes and thickness of the GQDs layer. The PCE of the solar cell significantly boosts from 7.99% to 10.67% as the GQDs layer thickness increases from 8 nm to 20 nm. Further increment of the GQDs layer thickness to 50 nm decreases the solar cell efficiency. The PCE of GQDs/Si heterojunction solar cells was 8.46%, 9.21%, and 10.50% for GQDs with various sizes of 6–12, 5–8, and 3–6 nm, respectively (Fig. 7(c) and (h)). After optimizing the sizes and thickness of the GQDs layer, the PEC of the GQDs/Si heterojunction solar cells was further enhanced through doping. Both current and voltage parameters increased, elevating the solar cell efficiency (Fig. 7(i) and (j)). According to their result, the best PCE (12.35%) was recorded at an optimal thickness (20 nm). The best PCE (11.43%) was also achieved at an optimal size 3–6 nm, after HNO3 doping. Ruan, Kaiqun et al.114 manufactured flexible Gr/Si solar cells with highly flexible ultrathin c-Si substrates (Fig. 7(k)). They used a thin layer of poly(3-hexylthiophene) (P3HT) between graphene and ultrathin c-Si as an electron-blocking layer to stifle carrier recombination at the interface and achieved the PCE of 8.42% for a c-Si thickness of 40 μm (Fig. 7(l)).
Fig. 7 (a) Schematic diagram of the GQDs/Si device with Gr thin film. (b) and (c) J–V characteristics and EQE spectra of GQDs/Si devices manufactured with GQDs of various sizes. (d)–(f) AFM micrograph of GQDs film with different thicknesses of 8, 20, and 50 nm. (g) and (h) J–V characteristics and EQE spectra of GQDs/Si devices manufactured with GQDs of various thicknesses. (i) and (j) J–V characteristics of the GQDs/Si solar cell after HNO3 doping. Reproduced from ref. 113, with permission from Elsevier. (k) Schematic diagram of the flexible garphene/ultrathin c-Si solar cell. (l) J–V characteristics of solar cell with and without HNO3 doping. Reproduced from ref. 114, with permission from the Royal Society of Chemistry. |
Fig. 8 (a) The alteration of effective carrier lifetime of Si, Gr/Si, FG/Si and Gr/FG/Si samples estimated by microwave photo-induced conductance decay (MW-PCD). (b) The EQE spectra of Gr/Si and Gr/FG/Si solar cells. (c) The EQE spectra of device with HNO3 doping and TiO2 antireflection layer. Reproduced from ref. 115, with permission from Elsevier. (d) Schematic of the FLG plane Si solar cell in which the P3HT layer is sandwiched between the FLG film and Si substrate. (e) and (f) J–V characteristics and EQE spectra of 4-layer FLG-CH3-Si solar cells with various P3HT layer thicknesses. (g) and (h) J–V characteristics and EQE spectra of the FLG-CH3-Si solar cells with altered FLG layer numbers, the thickness of P3HT was set at 10 nm. Reproduced from ref. 116, with permission from the Royal Society of Chemistry. (i) J–V characteristics of pristine and HNO3 treatment, with and without a LiF interlayer. Reproduced from ref. 117, with permission from the Royal Society of Chemistry. |
Zhong, Mengyao et al.115 proposed a one-stage strategy for doping and interface engineering of Gr/Si solar cells by employing the FG as an insulator interlayer. The carrier recombination of the device can be stifled at the front surface of Si via the FG interlayer. Fig. 8(a) illustrates the effective minority carrier lifetime (MCL) mapping of Gr/Si and Gr/FG/Si samples. The MCL of the Gr-deposited Si is approximately 16.2 μs. The Gr/FG solar cell deposited on Si, however, exhibits a considerably higher MCL (almost 20.6 μs). The boost of MCL can increase the external quantum efficiency (EQE) spectrum of the device, as depicted in Fig. 8(b). The clear boost of EQE at the short-wavelength range reflects the decline of carrier recombination. As a result, the power conversion efficiency (PCE) of the device improves from 3.17% to 7.52% with the application of the FG layer in the solar cell. Moreover, an enhancement is recorded in the PCE of the solar cell (13.38%) upon doping with HNO3 and TiO2 antireflection layer compared to the original solar cell (7.52%) (Fig. 8(a) and (b)).
Zhang et al. and Xie et al.116 reported the high-efficiency graphene-flat Si Schottky junction solar cells through modifying the Si surface with a molecule monolayer as well as interface band engineering with organic film (P3HT) to control electron distribution from n-Si to the graphene P3HT layer (Fig. 8(d)). The thickness of the P3HT layer was attentively managed by modifying the solution concentration. Various layer thicknesses were tested to reach the best performance of the Gr/Si solar cells and decrease the surface recombination. The best efficiency was obtained at the P3HT thickness of 10–20 nm, where, Jsc, Voc, FF, and PCE significantly improved from 21.85 mA cm−2, 0.38 V, 0.510, and 4.24% for the solar cell without a P3HT layer to 28.99 mA cm−2, 0.50 V, 0.669, and 9.70% for the solar cell with a P3HT layer (10 nm) (Fig. 8(e) and (f)). In addition, the highest PCE of graphene planar Si solar cells was achieved through additional optimization of the number of graphene layers and doping. They reported the optimal PCE of 10.56% in the system having 5-layer FLG-P3HT (10 nm)-CH3Si (Fig. 8(g) and (h)).
Xu, Dikai et al.117 used a lithium fluoride (LiF) layer as an insulator to stifle the recombination at the back surface and improve the hole blocking effect. The back contact resistance and series resistance of Gr–Si solar cells significantly declined, resulting in a remarkable rise in the power-conversion-efficiency (PCE) of devices.
As a consequence, the PCE of 6.25% was obtained for pristine Gr–Si solar cells. The highest value (10.61%) was recorded after HNO3 chemical doping (Fig. 8(i)).
Im, Min Ji et al.129 succeeded in heavy p-doping of the graphene layer via sandwich doping on both the top and bottom sides. The bottom side of the solar cell was doped by benzimidazole (BI) through etching while its top surface was doped with HAuCl4 solution (Fig. 9(a)). A monolayer of graphene was transferred by chemical vapor deposition (CVD). The sandwich-doping strategy boosted the work function to 5.07 eV, showing a 0.61 eV improvement compared to the pristine graphene device.
Fig. 9 (a) Schematic diagram of the four types of the solar cell (pristine, top-side-doped, bottom-side-doped, and sandwich-doped graphene/silicon solar cells). (b) The work function. (c) Sheet resistance and (d) light transmittance of various doped graphene. (e) and (f) J–V characteristics of four types of the solar cell. Reproduced from ref. 129, with permission from American Chemical Society. (g) Light J–V characteristics of the solar cells (the inset shows the sample exposed to the SOCl2 and HNO3 vapor). Reproduced from ref. 130, with permission from the Royal Society of Chemistry. |
In addition, the sheet resistance of sandwich-doped graphene was 165.4 Ω sq−1, showing a 35.1% decline compared to the original graphene device. Thus, doping raised the conductivity (Fig. 9(b) and (c)). Fig. 10(d) compares the optical transmission of graphene devices in the wavelength range of 400–1000 nm. The optical transmittance values of pristine, top-surface-doped, bottom-surface-doped, and sandwich-doped graphene at 550 nm were 96.4%, 94.4%, 95.4%, and 93.1%, respectively. These modifications indicate slight light absorption by the adsorbed dopants. The sandwich-doping approach enhanced the work function of graphene at low RS with no notable decrease in optical transmittance (>90%). The power conversion efficiency of graphene–silicon solar cells having both sides-doped graphene was 10.02%, exhibiting a 334% enhancement compared to that of Schottky junction solar cells (SJSCs) (2.998%) composed of pristine graphene (Fig. 9(e) and (f)).
Fig. 10 (a) Schematics of graphene/n-Si solar cell and TFSA-doped solar cell. (b) J–V curves of the device. Reproduced from ref. 132, with permission from American Chemical Society. (c) Schematic design of Gr/P3HT/Si solar cell with two-layered antireflection coating. (d) Energy band structure of Gr/P3HT/Si solar cell. (e) J–V curves of the device after TFSA doping and an antireflection layer of TiO2/PDMS (illuminated for 1 hour). Reproduced from ref. 133, with permission from Wiley. (f) Schematic of the processes implicated in the fabrication of PFSA/HNO3/graphene/native oxide/Si solar cells. (g) J–V characteristics and (h) EQE spectra of the solar cell. Reproduced from ref. 135, with permission from Wiley. |
Xinming Li et al.130 examined the heavy p-type chemical doping by Thionyl chloride (SOCl2) and nitrate anions (HNO3) using a vapor technique. Their result indicated that doping improved the solar cell. Doping is a more effective strategy to decrease the sheet resistance and widen the work function of graphene for efficient charge separation and transport. The series resistance (Rs) of the solar cells declined from 54.41 to 47.43 Ω (a 13% drop) and from 49.58 to 26.84 U (a 46% decline), after SOCl2 and HNO3 treatments, respectively. Correspondingly, the solar energy conversion efficiency improved from 5.52% to 8.94% and 5.53% to 9.27% after SOCl2 and HNO3 doping. Therefore, nitrate ions were more useful for the chemical doping of graphene films compared to chlorine, as they decremented Rs, enhanced Voc and FF, and improved the conductivity of graphene layers, which also contributed to the improvement of the Schottky junction solar cells (Fig. 9(g)). Similarly, Cui et al.131 employed four volatile oxidants (HNO3, SOCl2, HCl, and H2O2) or improving the performance of devices. They put the formed graphene/Si solar cells above a vial having HNO3 (65 wt%), SOCl2 (99.5 wt%), HCl (36 wt%), or H2O2 (30 wt%) for 60 seconds.
The PCE was significantly improved after treatment by either of the four volatile oxidants. The result showed that SOCl2 doping led to the best PCE. A primary PCE (2.58%) of a solar cell (Voc = 412.10 mV, Jsc = 17.65 mA cm2, FF = 35.42%) could be raised to 5.95% (Voc = 547.78 mV, Jsc = 17.92 mA cm2, FF = 60.64%) after SOCl2 doping.
Concerning volatile oxidants, doping with organic polymer dopant bis-(trifluoromethanesulfonyl) amide TFSA is also an influential approach to enhancing the efficiency of graphene/Si solar cells. Miao et al.132 reported that TFSA could considerably improve the conductivity of graphene by p-doping (Fig. 10(a)). They indicated an enhancement in the PCE of the graphene/n-Si Schottky junction solar cell (8.6%) upon doping with TFSA compared to the original solar cell (1.9%) while the Jsc boosted from 14.2 to 25.3 mA cm2, Voc raised from 0.43 to 0.54 V (Fig. 10(b)).
Xu et al.133 reported high-performance Gr/n-type Si solar cells by employing a solution-processable poly(3-hexylthiophene-2,5-diyl) (P3HT) thin film placed between the Gr and n-type Si (n-Si) for doping the Gr layer (Fig. 10(c)). The large-surface monolayer graphene layers were deposited on a copper foil via the low-pressure chemical vapor deposition method. Fig. 10(d) illustrates a schematic energy band of the Gr/P3HT/Si solar cells. The large bandgap (≈2 eV)134 of P3HT does not affect sunlight transmission via the Gr/P3HT transparent cathode and contact with the n-Si (see Fig. 10(e)). The highest occupied molecular orbital of P3HT (−5.0 eV) is placed very near to the maximum of the valence band of n-Si (−5.17 eV), promoting the transport of photogenerated holes. The lowest unoccupied molecular orbital of P3HT (−3.0 eV) is considerably greater than the minimum value of the conduction band of n-Si (−4.05 eV), providing a large energy barrier for photoinduced electron transport to the Gr film. Such an electron blocking layer not only effectively reduces the leakage current but also greatly stifles the carrier recombination at the junction. In the case of light brightness, the photoinduced doping boosted the work function of Gr, thus, declining the energy band offset between Gr and P3HT, further modifying the Voc and FF of the device.
This layer boosted the work function and conductivity of the Gr layer, therefore, improving the Schottky barrier height of the device as the carrier recombination was quenched at the interface. This phenomenon can be attributed to photoinduced p-type (hole) doping under light illumination. After 1 hour of exposure to sunlight, the doping effect saturates and the PCE of Gr/P3HT/Si solar cells increased from 0.92% to 6.78%. The use of antireflection-based polydimethylsiloxane (PDMS) pyramid arrays, TiO2 nanoparticles, and also extra chemical doping (TFSA) on the opposite side of the Gr layer enhances the performance of Gr/P3HT/nSi solar cells, offering a power conversion efficiency of 12.95% with elevated stability (Fig. 10(e)).
Rehman, Malik Abdul et al.135 used acid-based graphene-Si macromolecular solar cells chemically doped with polymeric perfluorinated sulfonic acid (PFSA) macromolecules and nitric acid (HNO3) (Fig. 10(f)). They reported a high PCE of ∼9.27% with PFSA doping compared with an undoped device (7.64%). The highest PCE of 10.44% was achieved after co-doping with HNO3. PFSA macromolecular doping significantly declined the number of defects, made the graphene surface smooth and uniform, and effectively improved the open circuit voltage (Voc) from 0.500 to 0.521 V (Fig. 10(g) and (h)).
Lately, nano or microstructures have been extensively studied to improve the PCE of this type of solar cell. Therefore, the research works on the manufacturing of highly efficient nanostructured and microstructural graphene/Si solar cells are reviewed in this section. Recently, nanostructures or microstructures have been extensively studied to enhance the PCE of this type of solar cell.
For instance, Fan et al.157 used a silver-assisted etching process to fabricate silicon nanowire (SiNW) arrays; they deposited the graphene film onto the silicon nanowire (SiNW) array by a CVD method using nickel foils. According to Fig. 11(a)–(d) the SiNWs led to a remarkable decrease in reflectance. Upon irradiation, the graphene/SiNW solar cell showed a great photovoltaic response, accomplishing a PCE of 1.25% with a Voc, Jsc, and FF of 0.462 V, 9.2 mA cm−2, and 30%, respectively. Such a great response can be predominantly associated with two factors. The SiNWs offer an immediate and quick pathway to enhance the electrical hole collection and transport. Second, the SiNWs can increment light trapping and quench the reflection of the junction surface in the near-infrared range. Then, they used SOCl2 vapor to dope the graphene film to further increase the PCE of the solar cells to 2.86% (Fig. 11(e)).
Fig. 11 Schematics diagram of (a) Gr/flat Si and (b) Gr/SiNW junctions. (c) Reflectance spectra of flat Si, SiNWs, Gr/Si, and G/SiNWs. (d) SEM micrograph of SiNW array. (e) J–V characteristics of the G/SiNW device before and after chemical doping. Reproduced from ref. 157, with permission from American Chemical Society. (f) Schematic diagram of the polymer-deposited Gr/Si solar cells. (g) Transmittance spectra of PMMA-eliminated and PMMA-deposited (2000 rpm) graphene. (h) Reflectance spectra of PMMA-eliminated and PMMA-deposited graphene samples. (i) J–V characteristics of the PMMA-eliminated and PMMA-deposited Gr/Si solar cells before and after HNO3 doping. Reproduced from ref. 158, with permission from the Royal Society of Chemistry. |
Gun et al.158 reported a new approach by incorporating PMMA antireflection film into the Gr/Si solar cells. PMMA coatings generally serve as a protective layer in the graphene transfer process and are dismissed after the transfer process. But in this report, the PMMA was fixed on the graphene film and acted as an anti-reflection layer (Fig. 11(f)). Notably, the transmittance at 550 nm was estimated to be 96.0% with PMMA coatings. The antireflection effect of PMMA coating was also explored (Fig. 11(g) and (h)). The result indicates that the PCE of the HNO3-doped with the PMMA coating increased to 13.34% (Fig. 11(i)). The performance of graphene/Si solar cells with TiO2 was very lower than graphene/Si solar cells with PMMA coating.
Fallahazad et al.159 fabricated two types of rGO/Si solar cells to compare the effect of the flat silicon substrate and pyramidal silicon substrate on the performance of the final device (Fig. 12(a)). In this work, the reduced graphene oxide (rGO) layers were transferred on the pyramidal silicon substrate by the electrophoretic deposition (EPD) method. The EPD technique offers proper thickness control of the graphene layer at reasonable costs. Fig. 12(b) displays the FESEM micrographs of graphene layers on a pyramidal Si substrate. The outcomes demonstrated a decline in the reflectance of pyramidal silicon substrate from 23% to 14% in flat silicon substrate due to the increased light paths in different directions (Fig. 12(c)). The J–V characteristic curve of rGO/flat Si solar cells showed an open-circuit voltage (Voc) value of 0.35 V and a Jsc value of 4.32 mA cm−2, corresponding to efficiency (η) of 0.94%. The Voc, Jsc, and η of rGO/pyramidal Si are 0.37 V, 7.54 mA cm−2, and 1.76%, respectively (Fig. 12(d)). The enhancement in Voc and Jsc of rGO/pyramidal Si solar cell can be assigned to the light entrapment which led to a remarkable efficiency improvement. Furthermore, this enhancement can be also attributed to the inferior series resistance and elevated shunt resistance.
Fig. 12 (a) Schematic structure of rGO/pyramidal Si solar cell. (b) FE-SEM images of the graphene layer on the pyramidal Si. (c) Reflection spectra of rGO on planner and pyramidal Si substrates. (d) J–V curves of the devices based on planner and pyramidal Si substrates. Reproduced from ref. 159, with permission from Elsevier. (e) Schematic diagram of the graphene/SiHA solar cell. (f) SEM images of SiHA sample. (g) and (h) J–V curves and EQE spectra of the graphene/SiHA solar cells with different hole depths. (i) Absorption spectra of the sample with different hole depths. Reproduced from ref. 160, with permission from The Royal Society of Chemistry. (j) Schematic illustration of the TiO2–Gr–Si solar cell. (k) Optical reflectance of a Gr/Si solar cell before and after TiO2 coating. (l) J–V curves of a Gr/Si solar cell recorded in the initial state (without coating), after HNO3 treatment, and after combined TiO2 layer deposition and HNO3 doping. Reproduced from ref. 161, with permission from American Chemical Society. |
Xie et al.160 investigated the structure of the graphene/microhole array (SiHA) device in terms of functionality and stability (Fig. 12(e)). They used photolithography and reactive ion etching (RIE) to achieve soft textured microhole arrays and controlled etching. They also employed a chemical vapor deposition (CVD) method for coating graphene layers. They manufactured graphene/microhole array (SiHA) devices with different hole depths. Fig. 12(f) shows the SEM image of SiHA. The improvement in the Jsc and EQE (external quantum efficiency) can be assigned to the improved optical absorption of the SiHA due to its deeper holes (Fig. 12(g) and (h)). According to their results, the optimal hole depth in SiHA was 12.8 μm due to the significant improvement of both current and voltage (Fig. 12(g)). Moreover, the best EQE of graphene/microhole array (SiHA) device was 80% at 680 nm as a result of the optimal hole depth of 12.8 μm (Fig. 12(h)). The thick SiHA (12.8 μm) exhibited the maximum effective optical absorption (above 80%) at the wavelength range of 400–1000 nm (Fig. 12(i)). Increasing the hole depth to 12.8 μm significantly improved the light capturing ability of the solar cells. The combination of the micro-hole array with AuCl3 doping enhanced the PCE to 10.4%. Further, the mentioned system exhibited excellent stability and high efficiency even after 3 months of exposure to air. Concerning stability, nano or microstructures can be viable candidates for efficient graphene/Si solar cells.
Shi et al.161 used TiO2 as an antireflection layer in a solar cell configuration comprising an n-Si substrate at the bottom and a TiO2 layer on the top sandwiching graphene. The mentioned system was achieved by the CVD method (Fig. 12(j)). Upon the deposition of TiO2 colloidal solution on the active surface of the graphene/Si solar cell to shape a soft layer, the reflectance in 500–800 nm was decreased to ∼10% (Fig. 12(k)). Also, the Jsc was enormously boosted from 23.9 to 32.5 mA cm−2 after TiO2 deposition. The resulting HNO3-doped TiO2/graphene/Si solar cell indicated a Voc of 0.60 V, a FF of 73%, and an efficiency of 14.1% (Fig. 12(l)). The Voc and FF enhancement can be ascribed to HNO3 doping, while the Jsc enhancement is related to TiO2 coating. By optimizing two parameters (Jsc and Voc), the PCE of graphene/Si solar cells reached 14.1%. The device lost its stability after doping as its efficiency extremely declined from 14.1% to 6.5% after 20 days in the ambient air. Nevertheless, the TiO2-induced antireflection properties ideally maintained the Jsc at almost 32 mA cm−2 during the mentioned period. They re-doped the device by HNO3 vapor, and the efficiency of the re-doped solar cell reached 14.5%, higher than that of previous records.
Ding et al.162 manufactured a multi-color Gr/Si solar cell based on MgF2/ZnS antireflection layer and extremely thin and highly transparent graphene. The maximum refractive index of ZnS is almost 2.5, while the minimum refractive index of MgF2 is 1.4. Hence, the MgF2/ZnS double film can act as an effective anti-reflection layer for solar cell devices. In this research, MgF2/ZnS was sequentially deposited on the graphene/Si solar cell by the thermal evaporation method. Different structural colors can be reached with accuracy by tuning the thickness of the films. The multi-color Gr/Si PV devices indicated acceptable power conversion efficiency (PCE) in the range of 10.7–13.2%, which is related to the color of the devices. Therefore, by optimizing the MgF2/ZnS anti-reflection layer, the PCE of the device can rise to 14.6%. Their results indicated the significant potential of colorful Gr/Si solar cells for high-efficiency and low-cost PV modules.
Kim et al.163 manufactured graphene/Si Schottky junction solar cells based on a porous silicon substrate (Fig. 13(a)). The target of their work was to enhance the optical absorption and electrical properties of the device with porous silicon. For this purpose, porous silicon was formed by metal-assisted chemical etching. Various deposition times (td) (1 to 7 s) were adopted for the etching of silicon substrate. Fig. 13(b) illustrates the energy band diagram of the graphene/PSi/n-Si junction. We suppose that the Fermi level of PSi resides at the middle of the bandgap regardless of the doping level of the starting silicon. The fact that the pores are mainly formed at the spots of Si defects and dopants during MacEtch164 causes an effective decrease in the doping concentration. The bandgap energy of porous silicon is larger than that of flat silicon due to the quantum confinement in Si nanostructures.165,166 The results indicated that a maximum PCE of 3.52% can be obtained by the deposition time (td) of 5 s for the etching of silicon substrate (Fig. 13(c)–(e)). Co-doping with Au NPs and TFSA was also utilized to improve the PCE of the solar cells from 3.52% to 10.69%. The co-doping sufficiently improved the work function of graphene and reduced sheet resistance of graphene compared to single-doping (Au NPs or TFSA) which was efficient for separating and collecting the photo-induced electron–hole pairs in the solar cells (Fig. 13(f)).
Fig. 13 (a) Schematic illustration of graphene/PSi/n-Si solar cell with Au top contact and InGa bottom contact. (b) Energy band diagrams of the device. (c)–(e) J–V characteristics, reflectance, and EQE spectra of the devices with td from 0 to 7 s. (f) J–V characteristics, and (d) EQE spectra of the pristine, individually doped (Au NPs or TFSA), and co-doped graphene layers/PSi solar cells. Reproduced from ref. 163, with permission from the Royal Society of Chemistry. |
The effect of the thickness of the graphene layer on the PCE of graphene/Si solar cells has been also investigated. Rehman, Malik Abdul et al.167 reported that carrier recombination is diminished by optimizing the thickness of the graphene layer. They altered the thickness of the layer from 2 nm to 4 nm, and 8 nm by prolonging the deposition time from 2.5 to 3.5 and 4.5 h, respectively (Fig. 14(a)). The result showed a high PCE of 5.51% for the 4 nm-thick graphene device deposited on bare flat silicon (Fig. 14(b)). Moreover, the efficiency is strangely increased to 9.18% upon the deposition of PMMA and doping with HNO3. Therefore, the smooth area of direct deposition of graphene and adjustment of the thickness of carbon with rising growth time was confirmed.
Fig. 14 (a) AFM micrograph to illustrate various thicknesses of graphene directly grown for different growth durations. (b) J–V curves of optimized thickness graphene layer under light and dark, with the PMMA layer and with HNO3 doping. Reproduced from ref. 167, with permission from Elsevier. (c) Schematic demonstration of the split and recombination of carriers at the interface of SLM/Si and MLG/Si. (d) J–V characteristics and (e) EQE spectra of SLG/Si and MLG/Si solar cells before and after doping. Reproduced from ref. 169, with permission from Wiley. (f) Schematic illustration of graphene/PSi solar cells. (g) J–V characteristics, and (h) EQE spectra of graphene/PSi/n-Si solar cells with various Ln values (from 1 to 4). Reproduced from ref. 170, with permission from American Institute of Physics. |
According to ref. 168 the photovoltaic characteristics of the graphene/Si solar cells can be improved by incrementing the number of graphene layers. The result showed a steady enhancement of the PCE and short circuit current of the solar cell for less than 4 graphene layers. The mentioned parameters showed a decline when the number of graphene layers exceeded 4. The decrease in PCE is thought to be due to a decrement in the graphene permeability for more than 5 layers. Thus, the 4-layer graphene is a superlative promising material for the development of high-performance Schottky junction solar cells. The PCE of the 4-layer graphene solar cell can be enhanced by further alteration of the graphene sheet resistance and the series resistance of the devices through chemical doping.
Xinming Li et al.169 reported the extremely superior solar conversion capacity of multilayer graphene films despite their lower transparency and conductivity compared to their monolayer counterparts. The multi-layer graphene leads to a reasonable junction compared to single-layer graphene and stifles the recombination at the junction (Fig. 14(c)). Chemical doping with acid remarkably improved the conversion efficiency of the MLG/Si device from 4.98% to 9.63% due to the enhancement in charge separation and transport. Doping also improved the efficiency of the SLG/Si device but not as high as the doped MLG/Si device (Fig. 14(d) and (e)). In another report, Shin et al.170 examined the effect of layer number (Ln) of graphene on the efficiency of graphene/PSi solar cells due to its direct association with the efficiency of graphene/PSi solar cells (Fig. 14(f)). In general, the sheet resistance, work function, transmittance, and reflectance of graphene highly depend on Ln. The most considerable PCE of 4.35% was achieved for Ln = 2 in the pristine graphene/PSi/n-Si solar cell. Several metal chlorides were employed as dopants in MLG at Ln = 2 to promote and enhance the efficiency of the solar cells (Fig. 14(g) and (h)). The RhCl3-doped graphene/PSi solar cell offered the maximum PCE of 9.15% due to its considerable work function and relatively small sheet resistance.
Fig. 15 (a) Schematic configuration of the graphene/GaAs solar cell, Five groups of characteristic (b) PCE, (c) Voc, (d) Jsc, and (e) FF of the devices with various numbers of graphene layers. (f) J–V characteristics of the devices. Reproduced from ref. 171, with permission from Elsevier. (g) Schematic diagram of the TiO2-coated Gr-P3HT-GaAs solar cell after TFSA doping. (h) The structure of P3HT. (i) J–V characteristics of the Gr-P3HT-GaAs solar cell recorded in the initial state with TFSA doping and with TFSA doping/AR film. Reproduced from ref. 173, with permission from Elsevier. (j) Energy band diagrams of the graphene/h-BN/GaAs solar cell with Si QDs. (l) Schematic illustration of the graphene/h-BN/GaAs solar cell. (k) J–V characteristics of devices with Si QDs presented photo-induced doping. Reproduced from ref. 174, with permission from ref. 174©The Optical Society. |
He Hang et al.173 developed a highly-efficient GaAs/graphene solar cell by modifying the interface of the device with poly(3-hexylthiophene) (P3HT) as a hole transport layer (Fig. 15(g) and (h)). The Voc and Jsc of the device showed an increment due to the presence of the P3HT layer. Such an improvement can be assigned to the rise of the built-in barrier and the decrease in the carrier recombination at the Gr–GaAs junction. A Primary PCE of 6.84% can be achieved for the Gr–GaAs solar cell with a P3HT layer. Moreover, TiO2 anti-reflective film and chemical doping by bis (trifluoromethanesulfonyl)-amide were also employed in the device with a P3HT layer, which led to the PCE of 13.7% (Fig. 15(i)).
Li Xiaoqiang et al.174 compared the power conversion efficiency (PCE) of graphene/h-BN/GaAs with graphene/GaAs structure (Fig. 15(j)). The barrier height of graphene/GaAs heterojunction can be improved by the use of h-BN due to the improvement of Fermi level adjustment effect through the h-BN interface. Moreover, the h-BN layer can quench the static charge transfer process. Fig. 15(k) indicates the electronic band diagram and charge transfer of the Si QDs doped graphene/h-BN/GaAs solar cell. The PCE of the graphene/GaAs heterojunction is 6.51% which rose to 7.10% in the graphene/h-BN/GaAs structure with 5 layers of h-BN. Upon photo-induced doping into the heterojunction, the PCE of 10.18% was obtained in graphene/h-BN/GaAs compared to 8.63% of graphene/GaAs structure (Fig. 15(l)).
Given the history of Gr/Si solar cells, we highlight some suggestions and an effective approach to possible PCE improvements, which should be taken into consideration for the future development of Gr/Si solar cells. The Gr/Si solar cells are yet to suffer from the shortage of passivation techniques. In contrast, different surface passivation techniques have been broadly studied for traditional p–n junction solar cells, such as passivated emitter and rear cell (PERC), passivated emitter, and rear locally-doped (PERL). Therefore, this is a practical and the most suitable scenario that will significantly improve graphene solar cells in the future. Passivation strategies and materials with higher efficiency can be employed to the rear contact of Gr/Si solar cells. More effective passivation material such as silicon nitride can be employed for the rear contact of Gr/Si solar cells. However, it is worth noting that the thickness of the passivation layer should be optimized because a supremely thin film may not be sufficient for effective passivation, while a considerably thick film would impede the efficient collection of carriers.
On the other hand, since the PCE of solar cells is restricted by the recombination of carriers, a silicon substrate with a longer lifetime would be expected to improve the efficiencies. Within this context, an investigation of the impact of silicon doping concentration on Gr/Si solar cell efficiency can be helpful to improve the Gr/Si junction construction. Another approach focuses on the device area, which could be further boosted by combining nano and micro-textured silicon, as a promising way to improve the PCE of Gr/Si solar cells in the future. However, there have been no reports on this strategy so far. Pyramidal silicon alongside porous silicon is an appropriate structure that can act as an antireflective layer to resolve the problem of the high reflection coefficient in the silicon substrates. In general, the PCE of Gr/Si is still low compared to conventional p–n junction solar cells; however, it is interesting and worth noting that the laboratory PCE of graphene-based silicon solar cells is ∼18%. Furthermore, under ideal conditions and based on theory, the efficiency limits of graphene/silicon and graphene/GaAs solar cells are expected to be 25.5% and 27.5%, respectively.175 Therefore, an obvious outlook can be predicted according to percentages obtained from the theoretical findings. In conclusion, the PCE of graphene/silicon solar cells would be further elevated to a superior record if whole performance engineering is contained and manufacturing quality can be improved.