Open Access Article
Grzegorz
Szczepaniak
*ab,
Jaepil
Jeong‡
a,
Kriti
Kapil‡
a,
Sajjad
Dadashi-Silab
a,
Saigopalakrishna S.
Yerneni
c,
Paulina
Ratajczyk
ad,
Sushil
Lathwal
a,
Dirk J.
Schild
a,
Subha R.
Das
ae and
Krzysztof
Matyjaszewski
*a
aDepartment of Chemistry, Carnegie Mellon University, Pittsburgh, Pennsylvania 15213, USA. E-mail: gszczepa@andrew.cmu.edu; matyjaszewski@cmu.edu
bFaculty of Chemistry, University of Warsaw, Pasteura 1, 02-093 Warsaw, Poland
cDepartment of Biomedical Engineering, Carnegie Mellon University, Pittsburgh, Pennsylvania 15213, USA
dFaculty of Chemistry, Adam Mickiewicz University, Uniwersytetu Poznańskiego 8, 61-614 Poznań, Poland
eCenter for Nucleic Acids Science & Technology, Carnegie Mellon University, Pittsburgh, Pennsylvania 15213, USA
First published on 20th September 2022
Photoinduced atom transfer radical polymerization (photo-ATRP) has risen to the forefront of modern polymer chemistry as a powerful tool giving access to well-defined materials with complex architecture. However, most photo-ATRP systems can only generate radicals under biocidal UV light and are oxygen-sensitive, hindering their practical use in the synthesis of polymer biohybrids. Herein, inspired by the photoinduced electron transfer-reversible addition–fragmentation chain transfer (PET-RAFT) polymerization, we demonstrate a dual photoredox/copper catalysis that allows open-air ATRP under green light irradiation. Eosin Y was used as an organic photoredox catalyst (PC) in combination with a copper complex (X–CuII/L). The role of PC was to trigger and drive the polymerization, while X–CuII/L acted as a deactivator, providing a well-controlled polymerization. The excited PC was oxidatively quenched by X–CuII/L, generating CuI/L activator and PC˙+. The ATRP ligand (L) used in excess then reduced the PC˙+, closing the photocatalytic cycle. The continuous reduction of X–CuII/L back to CuI/L by excited PC provided high oxygen tolerance. As a result, a well-controlled and rapid ATRP could proceed even in an open vessel despite continuous oxygen diffusion. This method allowed the synthesis of polymers with narrow molecular weight distributions and controlled molecular weights using Cu catalyst and PC at ppm levels in both aqueous and organic media. A detailed comparison of photo-ATRP with PET-RAFT polymerization revealed the superiority of dual photoredox/copper catalysis under biologically relevant conditions. The kinetic studies and fluorescence measurements indicated that in the absence of the X–CuII/L complex, green light irradiation caused faster photobleaching of eosin Y, leading to inhibition of PET-RAFT polymerization. Importantly, PET-RAFT polymerizations showed significantly higher dispersity values (1.14 ≤ Đ ≤ 4.01) in contrast to photo-ATRP (1.15 ≤ Đ ≤ 1.22) under identical conditions.
ATRP is a reversible redox process, typically catalyzed by copper complexes.8,9 The control over radical propagation in Cu-catalyzed ATRP is provided via a reversible redox reaction (Fig. 1). First, the CuI/L catalyst (L is typically a polydentate amine ligand) reacts with the dormant C(sp3)–X polymer chain end through a concerted inner sphere electron transfer to form two species: a X–CuII/L deactivator and a propagating carbon-based radical. Then, in the reverse reaction, the propagating radical reacts with the X–CuII/L, recovering the active form of the catalyst (CuI/L) and the dormant chain end (C(sp3)–X).10–12 A limitation of ATRP, like any other RDRP technique is its sensitivity to oxygen, as both initiating and propagating radicals are quenched by oxygen. Furthermore, molecular oxygen can oxidize an ATRP catalyst to its inactive form, inhibiting polymerization. Therefore, normal ATRP requires strictly anaerobic conditions.13 The sensitivity of ATRP techniques to oxygen hinders their use under ambient conditions and necessitates deoxygenation by inert gas purging, freeze–pump–thaw cycles, or using a glovebox. As a result, ATRP methods are time-consuming and can be challenging for non-experts.
To address these challenges, many efforts have been made to increase oxygen tolerance in ATRP.14–16 Since, at the ATRP equilibrium, the concentration of CuI/L is much higher than the concentration of propagating radicals, oxygen predominantly oxidizes CuI/L rather than reacting with radicals. This inspired researchers to harness CuI/CuII catalysis to function also as an oxygen scavenger.17–22 The continuous reduction of CuII/L back to CuI/L makes the ATRP inherently resistant to oxygen (Fig. 1).14 The alternative approach is based on adding glucose oxidase enzyme that removes oxygen without affecting the polymerization process, as in enzyme-assisted ATRP techniques.23–26 Despite these great improvements, most modern ATRP techniques tolerate only a limited amount of oxygen and can be performed in sealed vessels.22,27–31 When an open reaction vessel is used, the regeneration of the catalyst is usually slower than oxygen diffusion into the reaction site. To date, only a few ATRP systems are fully oxygen-tolerant and can be run in open-air reaction vessels.32–37
Photoinduced ATRP (photo-ATRP) techniques use light energy to generate activator CuI/L species, thus initiating polymerization.38–44 They typically require the use of biocidal UV light (<400 nm), which can degrade proteins, damage DNA, or initiate unwanted side reactions.45 Organocatalyzed ATRP (O-ATRP) relies on direct activation of the dormant polymer chain end by electron transfer from the photocatalyst in an excited state.46–52 It allows polymerization over a broad visible light spectrum,53–56 but moderate control and limited scope of monomers hinder its practical application, particularly under biologically relevant conditions.57 Dual catalytic ATRP systems use ppm-level copper catalysts to attain a controlled polymerization process in the ground state and photoredox catalysts (PCs) to reduce deactivators via photoinduced electron transfer, maintaining radical propagation.58–65 Moreover, when a PC in the excited state has sufficient redox potential, it can react directly with a dormant C(sp3)–X polymer chain end, generating radicals and thus offering an additional activation pathway. These methods are highly efficient under long-wavelength light, but have limited oxygen tolerance.
Another powerful photochemically driven RDRP technique is the photoinduced electron transfer RAFT (PET-RAFT) polymerization method developed by Boyer and co-workers.66 In the PET-RAFT, an excited PC can transfer energy/electrons to a chain transfer agent (CTA), generating propagating radicals.67–69 As in the conventional RAFT process, control over polymerization is provided by a CTA via a degenerative chain transfer mechanism.3 PET-RAFT can be used to polymerize a wide range of monomers, is oxygen tolerant, and exhibits perfect temporal control. Initially, PET-RAFT was performed using tris(phenylpyridinium) iridium(III) catalyst.66 The method was later expanded to several other photoredox systems, allowing polymerization under longer wavelength light.70–76 Eosin Y is one of the most widely used photocatalysts,77–79 especially for biological applications, due to its solubility in water, low toxicity, and cost. PET-RAFT catalyzed by eosin Y has recently been used to engineer protein and cell surfaces.45,80
Here, we demonstrate a dual photoredox/copper catalysis that enables ATRP under green light irradiation (Fig. 1). Inspired by PET-RAFT polymerization, we used eosin Y as the PC. In this dual catalytic system, control over radical propagation is provided by ATRP equilibrium, while eosin Y is essential for triggering and maintaining polymerization. In addition, the dual photoredox/copper catalysis removes oxygen, enabling the rapid open-to-air synthesis of well-defined polymers in both aqueous and organic media, outperforming PET-RAFT under identical conditions.
![]() | ||
| Fig. 2 (A) Reductive quenching vs. oxidative quenching cycle, (B) formation of EY in PBS solution, (C) proposed mechanism. | ||
Photo-ATRP was first attempted using molar ratios of [OEOMA500]/[HOBiB]/[CuBr2]/[TPMA] = 200/1/0.2/0.6. As expected, no OEOMA500 conversion, as measured by 1H NMR, was observed in the absence of the photoredox catalyst (entry 1, Table 1). O-ATRP catalyzed with the EY/TPMA (without CuBr2) enabled rapid polymerization, reaching 89% monomer conversion within 30 min (entry 2, Table 1),56 but size exclusion chromatography (SEC) analysis showed that the polymer had a high dispersity (Đ) of 4.30. On the other hand, when EYH2 was used in combination with CuBr2 and excess TPMA ligand, high monomer conversion (88%) and well-controlled polymerization (Đ = 1.19) were achieved (entry 3, Table 1). These experiments confirmed the critical role of dual catalysis in ensuring a well-controlled polymerization under green light irradiation.
| No. | EYH2 (equiv) | CuBr2 (equiv) | TPMA (equiv) | rpmb | Conv.c (%) | M n,th | M n,abs | M n,app | Đ |
|---|---|---|---|---|---|---|---|---|---|
| a Reactions conditions: [OEOMA500]/[HOBiB]/[EYH2]/[CuBr2]/[TPMA] = 200/1/x/x/x, [OEOMA500] = 300 mM, in PBS with DMSO (10% v/v), irradiated for 30 min under green LEDs (520 nm, 9.0 mW cm−2) in an open vial with stirring at 0–1000 rpm. b Revolutions per minute (rpm). c Monomer conversion was determined by using 1H NMR spectroscopy. d Molecular weight (Mn,abs) was determined by Mark–Houwink calibration. e Apparent molecular weight (Mn,app) and dispersity (Đ) were determined by GPC analysis (DMF as eluent) calibrated to poly(methyl methacrylate) standards. | |||||||||
| 1 | — | 0.2 | 0.6 | 0 | 0 | — | — | — | — |
| 2 | 0.05 | — | 0.6 | 0 | 89 | 89 000 |
187 500 |
126 000 |
4.30 |
| 3 | 0.05 | 0.2 | 0.6 | 0 | 88 | 88 000 |
84 000 |
65 000 |
1.19 |
| 4 | 0.05 | 0.2 | 0.6 | 250 | 86 | 86 000 |
82 500 |
64 000 |
1.18 |
| 5 | 0.05 | 0.2 | 0.6 | 500 | 86 | 86 000 |
86 000 |
66 000 |
1.15 |
| 6 | 0.05 | 0.2 | 0.6 | 1000 | 86 | 86 000 |
86 000 |
66 000 |
1.18 |
| 7 | 0.1 | 0.2 | 0.6 | 500 | 89 | 89 000 |
89 500 |
68 500 |
1.20 |
| 8 | 0.01 | 0.2 | 0.6 | 500 | 84 | 84 000 |
79 500 |
62 000 |
1.15 |
| 9 | 0.005 | 0.2 | 0.6 | 500 | 80 | 80 000 |
73 000 |
58 000 |
1.16 |
| 10 | 0.01 | 0.3 | 0.6 | 500 | 74 | 74 000 |
70 000 |
56 000 |
1.14 |
| 11 | 0.01 | 0.1 | 0.6 | 500 | 92 | 92 000 |
90 500 |
69 000 |
1.21 |
| 12 | 0.01 | 0.2 | 0.4 | 500 | 77 | 77 000 |
61 000 |
50 000 |
1.19 |
| 13 | 0.01 | 0.2 | 1.2 | 500 | 91 | 91 000 |
90 500 |
69 000 |
1.16 |
To evaluate oxygen tolerance, the stirring rate was increased from 0 to 250, 500, and 1000 rpm (entries 4–6, Table 1). All polymerizations were successful, yielding well-defined polymers with low dispersity (Đ < 1.18) and controlled molecular weights, indicating that the EY/Cu system is highly tolerant to increased oxygen mass transfer.
The amount of EYH2 was then varied to explore the performance of the dual catalytic system (entries 7–9, Table 1). Increasing the EYH2 concentration from 75 μM to 150 μM resulted in 89% monomer conversion and slightly higher dispersity (Đ = 1.20; entry 7, Table 1). In contrast, a 5-fold decrease in EYH2 concentration to 15 μM caused only a slight decrease in conversion (84%) while improving control over the polymerization (Mn,th = 84
000, Mn,abs = 79
500, Đ = 1.15; entry 8, Table 1). After further reduction of EYH2 to 7.5 μM (25 ppm relative to the monomer), the dual EY/Cu catalysis still provided a well-controlled polymerization (Đ = 1.16) with predetermined molecular weight (Mn,th = 80
000, Mn,abs = 73
000) and high monomer conversion of 80% (entry 9, Table 1).
Finally, the effect of CuBr2 and TPMA ligand concentrations was investigated (entries 10–13, Table 1). Increasing the amount of copper diminished the polymerization rate while improving its control (conv. = 74%, Đ = 1.14; entry 10, Table 1). Increasing the ligand concentration led to higher monomer conversion (conv. = 91%) and dispersity of 1.16 (entry 13, Table 1).
The free energy of a photoinduced electron transfer can be determined using the Gibbs energy of photoinduced electron transfer equation:
| ΔGet (eV) = −[E1/2(A/A˙−) − E1/2(D˙+/D)] − EPC* + ΔE |
| ΔGet (eV) = −[E1/2(CuIIL/CuIL) − E1/2(EY˙+/EY)] − EEY* |
| ΔGet (eV) = −[E1/2(EY/EY˙−) − E1/2(L˙+/L)] − EEY* |
In the EY/Cu dual catalysis, both CuI/L and 3EY* can react with molecular oxygen (E1/2(O2/O2˙−) = −0.87 V vs. SCE). The continuous regeneration of the CuI/L activator by EY provides high oxygen tolerance (Fig. 2C). The control over radical propagation is achieved through a reversible redox equilibrium between Cu(I) and Cu(II) complexes, where they act as intermittent activators of dormant species and deactivators of radicals. EY and the ligand used in excess are essential to initiate and sustain green light-induced polymerization in the presence of oxygen.
First, photo-ATRP was performed under optimized conditions ([OEOMA500]/[HOBiB]/[EYH2]/[CuBr2]/[TPMA] = 200/1/0.01/0.2/0.6) at a stirring rate of 500 rpm in an open vial. Kinetic analysis revealed a linear relationship between ln([M]0/[M]t) and time with a short induction period of 5 min, followed by a rapid polymerization that reached 91% monomer conversion within 40 min (Fig. 3A). In addition, the molecular weights increased as a function of monomer conversion, and molecular weight distribution values remained low (Đ ≤ 1.16) during the reaction (Fig. 3B and C).
![]() | ||
| Fig. 3 Polymerization kinetics of OEOMA500, (A–C) EY/Cu mediated photo-ATRP and (D–F) EY-catalyzed PET-RAFT polymerization. (G) EY fluorescence intensity measurements. | ||
Next, PET-RAFT polymerization of OEOMA500 was performed under identical conditions using 4-cyano-4-(phenylcarbonothioylthio)pentanoic acid (CPADB) as the CTA, EY as the photoredox catalyst and TEOA (TEOA = triethanolamine) as the sacrificial electron donor with [OEOMA500]/[CPADB]/[EYH2]/[TEOA] molar ratios of 200/1/0.01/0.6. Similar to photo-ATRP, a short induction period of 5 min was observed, followed by rapid polymerization, which reached 71% monomer conversion within 20 min (Fig. 3D). However, no further increase in conversion was observed over time. Fluorescence intensity measurements showed an 85% decrease in EY fluorescence after 30 min of PET-RAFT polymerization, while only 6% of the initial amount of EY was photobleached in photo-ATRP (Fig. 3G). The better performance of the EY/Cu dual catalysis can be attributed to the rapid electron transfer from 3EY* to CuII/L complex, increasing the long-term stability of EY under green light irradiation. In the absence of a CuII/L, EY degrades faster, leading to the inhibition of PET-RAFT polymerization. In addition, PET-RAFT polymerizations generated polymers with significantly higher dispersity values (Đ ≤ 1.45) (Fig. 3E and F), in contrast to photo-ATRP (Đ ≤ 1.16).
| No. | [OEOMA500]/[HOBiB]/[EYH2]/[CuBr2]/[TPMA] | [HOBiB] (mM) | Conv.b (%) | M n,th | M n,abs | M n,app | Đ |
|---|---|---|---|---|---|---|---|
| a Reaction conditions [OEOMA500] = 300 mM, [HOBiB] = 6.0–0.3 mM, [EYH2] = 15 μM, [CuBr2] = 0.3 mM, [TPMA] = 0.9 mM in PBS with DMSO (10% v/v), irradiated for 30 min under green LEDs (520 nm, 9.0 mW cm−2) in an open vial with stirring at 500 rpm. b Monomer conversion was determined by using 1H NMR spectroscopy. c Molecular weight (Mn,abs) was determined by Mark–Houwink calibration (see ESI). d Apparent molecular weight (Mn,app) and dispersity (Đ) were determined by GPC analysis (DMF as eluent) calibrated to poly(methyl methacrylate) standards. | |||||||
| 1 | 50/1/0.0025/0.05/0.15 | 6.0 | 74 | 18 500 |
16 500 |
17 000 |
1.22 |
| 2 | 100/1/0.005/0.1/0.3 | 3.0 | 81 | 40 500 |
38 000 |
34 000 |
1.16 |
| 3 | 200/1/0.01/0.2/0.6 | 1.5 | 84 | 84 000 |
79 500 |
62 000 |
1.15 |
| 4 | 400/1/0.02/0.4/1.2 | 0.75 | 79 | 158 000 |
179 000 |
121 000 |
1.16 |
| 5 | 600/1/0.03/0.6/1.8 | 0.5 | 73 | 219 000 |
305 000 |
188 000 |
1.16 |
| 6 | 800/1/0.04/0.8/2.4 | 0.325 | 68 | 272 000 |
483 000 |
275 000 |
1.15 |
| 7 | 1000/1/0.05/1.0/3.0 | 0.3 | 69 | 345 000 |
607 000 |
332 000 |
1.15 |
PET-RAFT polymerizations were then performed under identical conditions (Table 3). The target DP was set by adjusting the CTA concentration, while the concentrations of the other reagents were fixed for all experiments. The results showed an increase in molecular weight distribution values with increasing DPT (entries 1–7, Table 3 and Fig. 4B). In addition, significant deviations from the theoretical molecular weights were observed. Only for DPT = 100, the polymerization was well controlled (Mn,abs = 32
000, Đ = 1.14). The loss of control over polymerization could be attributed to a very low CTA concentration. Similar to photo-ATRP, a CTA can react with oxygen in the initial phase of the reaction, resulting in its degradation. In the case of RAFT, a CTA not only determines the initial target polymer chain length but is also responsible for the degenerative chain transfer process. In ATRP, control over polymerization is provided by a CuII/L deactivator, which is resistant to oxygen. In addition, Cu catalysis increases the tolerance of ATRP to oxygen since CuI/L species can scavenge oxygen. Therefore, in ATRP, deviations from theoretical molecular weights are observed for higher targeted DTT (entries 5–7, Table 2). At the same time, control over polymerization is not affected, demonstrating the superiority of EY/Cu dual catalysis. Interestingly, for the highest concentration of the CTA (6.0 mM, DPT = 50), no OEOMA500 conversion was observed (entry 1, Table 3). This could be explained by the insufficient loading of the photoredox catalyst. In contrast, under the same conditions, photo-ATRP reached 74% monomer conversion and low dispersity (Mn,abs = 16
500, Đ = 1.22, entry 1, Table 1).
| No. | [OEOMA500]/[CPADB]/[EYH2]/[TEOA] | [CPADB] (mM) | Conv.b (%) | M n,th | M n,abs | M n,app | Đ |
|---|---|---|---|---|---|---|---|
| a Reaction conditions [OEOMA500] = 300 mM, [CPADB] = 6.0–0.3 mM, [EYH2] = 15 μM, [TEOA] = 0.9 mM in PBS with DMSO (10% v/v), irradiated for 30 min under green LEDs (520 nm, 9.0 mW cm−2) in an open vial with stirring at 500 rpm. b Monomer conversion was determined by using 1H NMR spectroscopy. c Molecular weight (Mn,abs) was determined by Mark–Houwink calibration (see ESI). d Apparent molecular weight (Mn,app) and dispersity (Đ) were determined by GPC analysis (DMF as eluent) calibrated to poly(methyl methacrylate) standard. | |||||||
| 1 | 50/1/0.0025/0.15 | 6.0 | 0 | — | — | — | — |
| 2 | 100/1/0.005/0.3 | 3.0 | 53 | 28 000 |
32 000 |
29 500 |
1.14 |
| 3 | 200/1/0.01/0.6 | 1.5 | 75 | 75 000 |
82 500 |
64 000 |
1.42 |
| 4 | 400/1/0.02/1.2 | 0.75 | 58 | 116 000 |
98 500 |
74 000 |
1.68 |
| 5 | 600/1/0.03/1.8 | 0.5 | 50 | 150 000 |
108 000 |
80 000 |
2.52 |
| 6 | 800/1/0.04/2.4 | 0.325 | 51 | 204 000 |
98 500 |
74 000 |
3.63 |
| 7 | 1000/1/0.05/3.0 | 0.3 | 50 | 250 000 |
115 000 |
84 000 |
4.01 |
500, Đ = 1.20). A sample was then taken from the post-polymerization mixture and used without further purification to prepare an ATRP “cocktail” with OEOMA300 monomer (DPT = 250). After 30 min of green light irradiation, the monomer conversion was 70%. SEC analysis showed a clear shift toward higher molecular weights without any shoulder or tailing at lower molecular weights (Mn,app = 51
000, Đ = 1.18), indicating well-controlled polymerization and high retention of chain-end fidelity.
To investigate the low volume performance of the EY/Cu system, a series of reactions at volumes of 250, 150, and 50 μL were performed in open reaction vessels (Table S1†). Polymerizations were carried out with [OEOMA500]/[HOBiB]/[EYH2]/[CuBr2]/[TPMA] molar ratios of 1000/1/0.05/1/3. Despite the reduced volume and target DP of 1000, high monomer conversions (72–80%) were achieved in all reactions, and only for a volume of 50 μL the polymerization was less controlled (Đ = 1.46, entry 4, Table S1†).
These results indicate the great potential of this technique for high-throughput screening applications.
The dual EY/Cu system was applied in protein modifications. First, ATRP initiators were covalently attached to the accessible lysine residues in bovine serum albumin (BSA) to yield the protein macroinitiator BSA-[iBBr]22. The model protein–polymer bioconjugate was then prepared by grafting polymer chains from the surface of BSA using molar ratios of [OEOMA500]/[BSA-iBBr22]/[EYH2]/[CuBr2]/[TPMA] = 400/0.045/0.02/0.4/0.8 (Fig. 4E). Within 25 minutes, 45% monomer conversion was reached. SEC with multi-angle light scattering (MALS) analysis confirmed the well-controlled synthesis of the protein–polymer hybrid (Mn,th = 1
848
000, Mn,MALS = 1
864
000, Đ = 1.28, Fig. S3†).
Nucleic acid–polymer conjugates represent another important class of biohybrids used as multifunctional biomaterials in nanoscience and biomedicine.91,104,108–110 Therefore, we decided to use the EY/Cu technique to graft polymers from DNA. A 23-mer DNA-based macroinitiator (DNA-iBBr) with α-bromoisobutyrate group at the 5′-end was prepared in a DNA synthesizer111 and then extended with OEOMA500, and molar ratios of [OEOMA500]/[DNA-iBBr]/[EYH2]/[CuBr2]/[TPMA] = 600/1/0.03/0.6/1.8 at a low reaction volume of 250 μL (Fig. 4F). After 30 min of green light irradiation, 76% monomer conversion was achieved. SEC-MALS analysis showed that the DNA-polymer biohybrid had a dispersity of 1.04, and absolute molecular weight close to the theoretical value (Mn,th = 231
000, Mn,MALS = 259
500, Fig. S4†), indicating a well-controlled polymerization.
It is a common belief that Cu-catalyzed ATRP methods are more cytotoxic than metal-free RAFT techniques. The cytocompatibility of EY/Cu dual catalysis was investigated and compared with EY-catalyzed PET-RAFT (Fig. 4G). Polymerizations were performed in the presence of human embryonic kidney 293 (HEK293) cells at a low volume of 250 μL using a 96-Well LED array (520 nm, 25 mW cm−2). The cells tolerated both the ATRP and RAFT polymerization in vitro at a similar level. Compared to the control (untreated cells), 81% of the cells exposed to photo-ATRP for 10 min remained viable vs. 85% in PET-RAFT, indicating that the EY/Cu-catalyzed ATRP technique can be utilized in live cell surface engineering.
100, Mn,abs = 14
300). Further reduction of the amount of EYH2 improved monomer conversion (84%), but formed polymer with the dispersity of 1.07 and deviation from the theoretical molecular weight value (Mn,th = 14
600, Mn,abs = 12
200). Despite reducing CuBr2 to just 100 ppm (relative to monomer), the ATRP was well-controlled (Đ = 1.08). Importantly, reducing EYH2 5-fold to just 1 ppm still allowed polymerization of MA (entry 5, Table 4). However, the monomer conversion dropped to 44%, and the dispersity increased to 1.23.
| No. | [EYH2] (equiv) | CuBr2 (equiv) | Me6TREN (equiv) | Conv.b (%) | M n,th | M n,abs | M n,app | Đ |
|---|---|---|---|---|---|---|---|---|
| a Reaction conditions: [MA]/[MBiB]/[EYH2]/[CuBr2]/[Me6TREN] = 200/1/x/x/x, [MA] = 5.5 M, in DMSO, irradiated for 60 min under green LEDs (520 nm, 9.0 mW cm−2) in an open vial with no stirring. b Monomer conversion was determined by using 1H NMR spectroscopy. c Molecular weight (Mn,abs) was determined by Mark–Houwink calibration. d Apparent molecular weight (Mn,app) and dispersity (Đ) were determined by GPC analysis (THF as eluent) calibrated to poly(methyl methacrylate) standards. | ||||||||
| 1 | 0.01 | 0.05 | 0.3 | 48 | 8500 | 17 200 |
21 000 |
1.12 |
| 2 | 0.005 | 0.05 | 0.3 | 81 | 14 100 |
14 300 |
17 300 |
1.05 |
| 3 | 0.001 | 0.05 | 0.3 | 84 | 14 600 |
12 200 |
14 600 |
1.07 |
| 4 | 0.001 | 0.02 | 0.12 | 79 | 13 800 |
11 500 |
13 700 |
1.08 |
| 5 | 0.0002 | 0.02 | 0.12 | 44 | 7800 | 8300 | 9800 | 1.23 |
Footnotes |
| † Electronic supplementary information (ESI) available. See https://doi.org/10.1039/d2sc04210j |
| ‡ J.J. and K.K. contributed equally to this work. |
| This journal is © The Royal Society of Chemistry 2022 |