Laxman
Gouda
ab,
Laurent
Sévery
a,
Thomas
Moehl
a,
Elena
Mas-Marzá
b,
Pardis
Adams
a,
Francisco
Fabregat-Santiago
*b and
S. David
Tilley
*a
aDepartment of Chemistry, University of Zurich, Winterthurerstrasse 190, CH-8057 Zurich, Switzerland. E-mail: david.tilley@chem.uzh.ch
bInstitute of Advanced Materials (INAM), Universitat Jaume I, Avda. V. Sos Baynat s/n, 12006 Castelló de la Plana, Spain. E-mail: fabresan@uji.es
First published on 29th September 2021
Electrochemical reactions powered by renewable electricity are an important means of reducing the carbon footprint of large-scale chemical processes. Here, we investigate the efficient conversion of biomass-derived 5-hydroxymethylfurfural (HMF) to 2,5-furandicarboxylic acid (FDCA), an important building block in the polymer and pharmaceutical industries, using a cheap and abundant nickel-based electrocatalyst. We elucidate the key factors for tuning the chemical selectivity for HMF oxidation over the competing oxygen evolution reaction (OER) at the catalyst surface. We show that the selectivity for HMF oxidation is enhanced by removing trace impurities of iron species as well as adjusting the composition of the alkali hydroxide electrolyte solution. LiOH solution without iron impurities is more favorable for HMF oxidation, whereas CsOH solution with iron species present is more active for the OER and unfavorable for HMF oxidation. Under optimized conditions, HMF oxidation in 1 M LiOH electrolyte solution without iron (pH 14) achieved 98% faradaic efficiency for the production of FDCA. The principles used in this work can be applied to other electrosynthetic reactions, in particular where the OER is the main competing side reaction.
Regarding oxygen production, natural photosynthesis is sufficient to supply the global requirements of the chemical industry. Therefore, in electrolysis, instead of using the oxidation equivalents to drive the notoriously demanding OER (and yielding a low value product), the OER could be replaced by a useful alternative reaction leading to added-value products.3,9 One option for this alternative reaction is the oxidation of lignocellulosic biomass, an abundant and renewable chemical feedstock for many commodity chemicals.3,10 Among biomass-based commodity chemicals, 2,5-furandicarboxylic acid (FDCA) belongs to the most economically valuable ones.11 The biomass derived product FDCA is used to fabricate the polymer polyethylene furanoate (PEF). The properties of PEF are superior in many ways to those of the petrochemical-based polyethylene terephthalate (PET), such as lower melting point, higher glass transition temperature, better barrier properties to O2 and CO2, and 100% recyclability with reduced carbon footprint, which would enable the fabrication of lighter and better plastic containers and packagings.12–14 It is estimated that 30.3 million tons of PET are produced per year globally.12 Therefore, PEF has the potential to replace PET as a renewable alternative.15 The building block FDCA is synthesized from 5-hydroxymethylfurfural (HMF), which is derived from lignocellulosic biomass.16
There are several ways to convert HMF into FDCA, such as aerobic oxidation, thermal treatment, and high temperature catalytic oxidation. These methods are sufficient to reach a large industrial scale, although the long processing time, high operating temperatures, and by-product formation make these processes cost-inefficient.16,17 An alternative approach is electrochemical oxidation, where HMF oxidation is driven by electrical potential, eliminating the use of chemical oxidants for the process.18 Considering its potential for low cost, high yield and the scalability of this method, the electrocatalytic approach to biomass oxidation has attracted notable attention.19 Electrosynthesis coupled with HER presents an elegant solution to provide renewable hydrogen for the chemical industry along with the synthesis of valuable biomass-derived chemical products.10,20
As early as 1991, electrocatalytic oxidation of HMF to FDCA was first reported by Grabowski and co-workers.21 Typically, electrochemical HMF oxidation is performed in basic media and can take place over two distinct reaction pathways, as shown in Scheme 1.16 It has been reported that electrochemical HMF oxidation in aqueous solution competes with water oxidation under the required operating potentials, resulting in relatively low FDCA yields.22 To circumvent competition with the OER, redox mediators such as TEMPO ((2,2,6,6-tetramethylpiperidin-1-yl)oxyl) have been used for indirect HMF oxidation, with excellent conversion efficiencies.20 However, the use of organic redox mediators is considered to be cost-prohibitive on industrial scale. As an alternative, nickel (and its corresponding oxides and hydroxides, specifically nickel oxide hydroxide NiO–OH) is a cheap, abundant and widely explored redox catalyst for alcohol oxidation reactions.23 The first reported electro oxidation of HMF with NiO–OH gave only 71% FDCA yield at pH 14, however subsequent advancement in the NiO–OH chemistry, gave more than 90% FDCA yield.21,24 NiO–OH is also a good water oxidation catalyst, and therefore a strategy that favors the organic oxidation reaction (alcohol and aldehyde functional groups oxidation) over the OER is required.25 There are two main strategies reported in the literature to tune the selectivity: tailoring the electrolyte composition and electrolysis conditions, or altering the nickel surface structure with different starting materials (i.e. NiP, NiS and NiFe).10,26–28 In any case, the main active species in Ni based catalysts is amorphous β-NiO–OH.24,25,29
Most of the organic oxidation reactions using NiO–OH are reported at pH > 11, where this catalyst also has optimal activity for the OER reaction.30 Although the overpotential for the HMF oxidation reaction can be much higher than for the OER, it is thermodynamically easier, and therefore selective HMF oxidation over the OER can be achieved.31,32 The OER onset of NiO–OH can be tuned by varying the electrolyte solution composition with different cations (Cs+, K+, Na+ and Li+) as well as by incorporating iron into the catalyst, transforming the NiO–OH to Ni1−xFexOOH.33–37 Thus, the competition between the two electrochemical oxidation reactions at the NiO–OH surface can be tuned by controlling the traces of iron and the alkali metal cation in the electrolyte solution.
Our simple approach uses an electrodeposited Ni(OH)2 film as a precursor to study the NiO–OH electrode systematically for HMF oxidation, under strongly basic conditions. We performed in situ studies to explore HMF oxidation vs. self-degradation as well as the selectivity between HMF oxidation and the competing OER. The key finding is that removal of traces of iron from the electrolyte solution enables high chemical selectivity of HMF oxidation over water oxidation, which enables the practical use of earth abundant Ni-based anodes in aqueous electrochemical cells targeting oxidation of organic molecules. High chemical selectivity of NiO–OH for HMF oxidation over water oxidation can be then achieved by smaller alkali cations in combination with an electrolyte solution free of traces of iron.
A typical cyclic voltammetry (CV) measurement under stirring of a NiO–OH electrode after activation in the standard iron-free electrolyte solution (1 M LiOH) is shown in Fig. 2a (black line). The main features in this CV are the Ni2+/Ni3+ redox peak between 1.2 to 1.4 V and the OER onset at 1.6 V vs. RHE (with ∼350 mV overpotential at a current of 0.1 mA cm−2, see also Fig. S4†).29,35 A broad oxidation peak is also visible at around 1.8 V, which corresponds to the higher oxidation state Ni3+/Ni4+.35 Upon addition of HMF, an oxidative wave appears with a peak at 1.47 V vs. RHE, merging with the OER at more positive potentials (Fig. 2a; red trace). After 300 CV scans, the HMF oxidation peak is no longer visible (Fig. 2a; green trace), indicating nearly complete consumption or degradation of the substrate (vide infra for details in the quantification of products). The consecutive CVs in Fig. 2b show that after the reaction, the Ni2+/Ni3+ redox peak has shifted to slightly more positive potentials (by ∼50 mV) while the OER shows an earlier onset potential (∼50 mV).
Normally, trace impurities such as iron in the electrolyte solution can be adsorbed at the catalyst surface or, as reported, incorporated into the NiO–OH crystal lattice, which can lead to shifts in the OER onset and Ni redox peak.34,38,39 Since we used iron purified electrolyte for our experiments, the only source of iron impurities could be from the HMF. We therefore performed inductively coupled plasma mass spectroscopy (ICP-MS) of the HMF starting material. Indeed, we found that for a 5 mM solution of HMF, traces of iron were present at a concentration of 2.2 nM, which likely gives rise to the shift in the nickel redox peak.
To explore more about the observed peak shifts we additionally performed prolonged OER at 1.8 V vs. RHE with freshly prepared electrodes both with and without iron in the electrolyte solution. The electrolyte solutions “with iron” were prepared by adding intentionally a known amount of iron to iron-free electrolyte solutions (with a ratio of nickel to iron atoms of either ∼200 or ∼100 to 1 in contrast to the ratio of nickel to iron in the iron purified electrolyte solution of at least 4700:1 (see Experimental section in ESI and Table S1†). The NiO–OH redox peak in iron-free electrolyte solution did not change its redox potential in this prolonged OER experiment while the OER showed only a minor shift to lower onset potential (Fig. S5a†). For the case with the intentionally added iron into the electrolyte solution (Fig. S5b†), we likewise did not observe a clear shift of the redox peak of Ni(OH)2/NiO–OH (2+/3+), although the onset of the OER in this case clearly shifted to a lower onset potential. Generally, the Ni2+/Ni3+ redox peak shift has been found to be very sensitive to iron concentration, microenvironments and deposition methods.40 The shift of the OER onset potential to more negative potentials is a clear indication of iron incorporation into the NiO–OH crystal lattice.40
Investigating the CVs further, another interesting observation is found. The oxidative wave for HMF at the NiO–OH surface occurs not only when scanning to more positive potentials but also on the negative sweep, which is unusual. A similar behavior has been observed with glucose oxidation on NiO electrodes.41,42 Though in the literature this is often only explained in terms of binding of an intermediate to the catalyst surface, a more sophisticated treatment of such observations can be found in oscillating electrochemical reactions.43–46 Generally, oscillating (electro)chemical reactions, like the Belousov–Zhabotinsky reaction, are based on an auto-catalytic step in the reaction mechanism itself. Such behavior can be described in more simplified reaction schemes/kinetics like the Bruesselator or the Oregonator.47,48 On the other hand oscillations in electrochemical reactions can also appear if the electrode or the catalyst surface and therefore the active sites for catalysis are blocked by reaction intermediates. Known examples include formic acid, formaldehyde, methanol, ethylene glycol, ethanol, glycerol or glucose and their oxidation on Pt.46 To verify the oscillating behavior of our electrochemical reaction, we performed slow galvanodynamic scans (50 nA s−1) and observed the evolution of the potential (Fig. S6†). Clearly potential oscillations were observed during the current scan, supporting our assumption.
This oscillatory behavior suggests a potential-dependent binding of HMF reaction intermediates that partially block the active sites on the catalytic surface and is consistent with our observation of the less-than-expected amount of substrate and product in the reaction solution under electrical polarization, shown in Fig. 3b (see discussion below). Furthermore, no cathodic reduction peak for the back reaction of FDCA or the intermediates to HMF was observed in the CV, indicating that the oxidation of HMF at the NiO–OH electrodes is an irreversible process.
The products formed during chronoamperometric studies were also quantified by UPLC and showed a similar trend as in the 1H-NMR spectra (Fig. S11†). Upon close inspection, one can observe both for the 1H-NMR and the UPLC measurements that initially the formation of FDCA is not 1:1 with respect to the amount of HMF converted. At the intermediate data points, obtained by sampling the solution during the electrolysis, the total concentration of HMF and of the products detected does not match the initial starting concentration. The last data point – obtained after stopping the electrolysis, releasing the potential, and equilibrating the electrolyte solution under continuous stirring – shows that all HMF has been transformed to either FDCA or formate. The amount of FDCA determined in this last datapoint of the UPLC suggests that partially oxidized HMF species and/or FDCA are trapped and accumulate at the electrode surface under applied potential as no peaks for intermediate species could be observed in the aliquots measured by 1H-NMR. This observation is also consistent with the unusual CV behavior shown in Fig. 2 and the oscillatory behavior shown in Fig. S6.†
As discussed earlier, traces of iron in electrolyte can interact with the NiO–OH catalyst and be incorporated into the catalyst structure, which promotes a synergetic effect on the OER.38 Based on the literature, the role of iron is still under debate. However, it is very well understood that iron incorporation reduces the covalent character of the Ni–O bonds, which energetically favors the adsorption of oxygen intermediates, and thus enhances molecular oxygen evolution.35,40 Therefore, iron traces at the NiO–OH matrix synergistically lowers the OER overpotential. In this scenario, the competing OER process reduces the HMF conversion on the NiO–OH surface. Based on these observations we can infer that iron-free LiOH should be the best choice for electrochemical HMF oxidation with a minimal contribution from the competing OER. Thus, we systematically investigated the chemical selectivity between electrooxidation of HMF and OER activity with varying alkali cations with and without traces of iron in the electrolyte solution. For clarity, we have plotted the electrochemical data using only the smallest and largest cation size with and without traces of iron in the electrolyte solution (Fig. 4). The comparison with all four alkali cations can be found in the ESI (Fig. S12 and S13†). We observe a shift in the OER onset with different alkali cation similar to a previous report (Fig. 4a and b).32 Thus, the presence of Li+ in the electrolyte solution leads to a higher OER overpotential as compared to Cs+. The shift in the OER onset follows the size of the cations used for the electrolyte solutions as can be observed in Fig. 4 and S12.† This is exemplified in the negative shift of the OER onset potential in the presence of iron and Cs+, appearing very close to the Ni2+/Ni3+ redox peak as shown in Fig. 4b and d. Fig. 4d shows that OER with Cs+ and HMF in solution is the dominant reaction under such conditions as compared to HMF oxidation. The trend of the alkali cation size favoring OER is clearly more pronounced with trace iron present and without HMF in solution (Fig. 4b and c and S13b and d†).
Interestingly, the hysteresis of the CV curve after OER onset (in the region from 1.6 V to 2 V) is clearly visible in the samples without iron. In the samples with iron, as the faradaic current increases, this effect is reduced until it is almost negligible. This fact could be related to some structural transformation of the catalyst, or the activation of the Ni3+/Ni4+ redox state.38 In any case, the potential interest of this process in the OER is beyond the scope of this study.
When adding HMF to the electrolyte solutions, similar CV features are observed as discussed above. The electrochemical potential at which HMF oxidation current appears following oxidation of the Ni2+/Ni3+ redox peak and remains at nearly the same potential for all the cations used. Meanwhile, the onset potential of the OER has an extra slight negative shift for all cation sizes. In the case of the electrolyte with Fe and of Cs+, the peak of the HMF oxidation is hardly visible, suggesting that in this case OER dominates the reaction. While addressing the overall scheme, it is remarkable that, (except for Li cation) the larger the cation, the narrower potential difference between Ni redox peak/HMF oxidation potential and OER onset potential is observed. Thus, Ni redox peak and HMF oxidation potential shifts to higher potential while the OER onset shifts to lower potential. This fact suggests that on the Ni surface the HMF oxidation and OER occur by two independent mechanisms. Further investigation is needed to fully understand the origin of these mechanisms.
To analyze the conversion performance of these different electrolyte solutions, chronoamperometric oxidation experiments were carried out for 20 hours with the different electrolyte solution compositions at 1.5 V vs. RHE, where HMF has highest oxidation current and OER current is small. The conversion efficiencies are presented in Table 1 and Table S2.† As the competing OER decreases with the smaller cation size, the faradaic efficiency of HMF to FDCA conversion increases, and we observe the highest faradaic efficiency (and chemical yield) with LiOH and the lowest with CsOH (Table S3†).
1 M electrolyte solution with | Faradaic efficiency without iron (UPLC) % | Faradaic Efficiency with iron (UPLC) % |
---|---|---|
LiOH | 98 | 90 |
NaOH | 95 | 88 |
KOH | 93 | 85 |
CsOH | 93 | <6 |
The data in Table 1 show that with traces of iron in the electrolyte solution, the OER can more easily compete with HMF oxidation and in the case of electrolyte solution containing cesium cation, the OER is in fact the dominant reaction at given applied potential (with only 6% FDCA formation). Thus, we observed a reduction in the faradaic efficiency for FDCA formation for all metal cations in the presence of iron impurities. Thus, while for LiOH the reaction still showed a high faradaic efficiency, for CsOH, the transformation to FDCA could not be completed and a variety of intermediate products such as HFCA, FFCA, and side products like formate and dimethylfuran were detected (Fig. S14 and Table S3†). Finally, our findings show that the faradaic efficiency (and chemical yield) change due to the variation of the alkali cation in the absence of trace iron in the electrolyte is small. However, the presence of trace iron activates the electrode for the competing OER the larger the alkali cation size is, lowering the yields and removing the possibility of selective HMF oxidation at any potential in the case of CsOH.
Footnote |
† Electronic supplementary information (ESI) available: Experimental details, HMF oxidation and OER reaction equations, AFM images of the electrodes, EDX measurements, CV of redox peaks of the nickel electrode, OER with and without iron, UPLC study of HMF oxidation, 1H-NMR spectra of HMF and its intermediates, 1H-NMR study of HMF degradation, 1H-NMR spectra of HMF oxidation for LiOH without iron and CsOH with iron, reaction mixture analysis by UPLC and 1H-NMR. See DOI: 10.1039/d1gc02031e |
This journal is © The Royal Society of Chemistry 2021 |