Xueke
Zhu
,
Dong
Fang
*,
Lang
Zhang
* and
Jianhong
Yi
Faculty of Materials Science and Engineering, Kunming University of Science and Technology, Kunming, 650093, P. R. China. E-mail: fangdong@kmust.edu.cn; 3086818048@qq.com
First published on 21st July 2025
The major challenges in using NH4V4O10 as a cathode for aqueous zinc-ion batteries (AZIBs) are its unsatisfactory structural stability and carrier migration coefficient due to the accumulated lattice strain during cycling. Herein, we developed a K0.16Na0.05(NH4)0.71V4O10−x·0.63H2O (NaKNVOH) cathode to achieve a continuous contribution of cathode structure for Zn2+ storage at both low and high current density. Both experimental data and DFT calculations confirmed that the charge compensation of Na+ and K+ not only reinforced the host structure but also enriched the active sites for Zn2+ migration. Especially, the structure-led charge compensation effectively alleviated the lattice strain accumulation during prolonged cycling. The NaKNVOH cathode delivered a specific capacity of 495.4 mAh g−1 at 0.5 A g−1, a rate capability of 177.8 mAh g−1 at 4 A g−1, and excellent cycle life and capacity retention at current densities of 0.5 A g−1 (300 cycles, 94.2%) and 4 A g−1 (2000 cycles, 96.57%).
To address this issue, significant efforts have been made to enhance the electrostatic interaction of the [VOn] skeleton and limit the invertible extraction of interlayered “pillars” through strategies such as the introduction of guest ions (K+, Na+, Ag+, Cu2+, and Al3+) or molecules (H2O and C3N4), construction of artificial cathode-electrolyte interface layer, and optimization of electrolytes.3,9–14 Among these, pre-intercalating hetero-cations have been shown to enhance the stability of the lattice structure and reduce the energy barrier in layered cathodes during electrochemical reactions.12,15 The regulation of the covalent degree's effect on the mean charge of lattice oxygen by pre-intercalated metal-ions, resulting in an improved Zn2+ diffusion kinetics. Particularly, alkali metal cations (M+, M = Li, Na, and K) endow NVO with tunable structural integrity and satisfactory electrochemical kinetics derived from their different ionic radii and masses.16,17 A previous work has demonstrated that the sole incorporation of K+ results in low electronic conductivity, leading to significantly inadequate rate capability. Concurrently, the relatively weak structural stability causes noticeable capacity fading during long-term cycling.16 Under this background, the charge compensation effect between dual cations (such as Na+ and K+) may effectively alleviate lattice strain accumulation during prolonged cycling, thereby significantly reducing the diffusion energy barrier of Zn2+ and promoting cycle stability at both high and low current densities.16–19
Herein, we developed a medium-entropy K0.16Na0.05(NH4)0.71V4O10−x·0.63H2O (NaKNVOH) nanowire by utilizing the regulatory effect of “Na+–K+-in-subsequence” for efficient Zn2+ storage. Unlike single Na+ ion intercalation, Na+–K+-in-subsequence expands the interlayer spacing and reduces the migration energy barrier, facilitating efficient Zn2+ transport. In addition, the charge compensation effect between Na+ and K+ effectively alleviates lattice strain. The NaKNVOH cathode delivers a high specific capacity of 336.0 mAh g−1 at 0.5 A g−1 with outstanding rate capability (177.8 mAh g−1 at 4 A g−1) and excellent cycling stability at current densities of 0.5 and 4 A g−1. Furthermore, the positive Zn2+/H+ migration mechanism in NaKNVOH has been confirmed by in situ XRD analysis and DFT calculation, which is of great significance for the construction of high-performance layered cathode for AZIBs.
000 Hz were recorded using an electrochemical workstation (CHI 760E, Shanghai Chenhua Company, PR China). The galvanostatic discharge charge (GDC) and the galvanostatic intermittent titration technique (GITT) were performed utilizing a battery test system (NEWARE, PR China). The capacity fluctuations during cycling arise from variations in the ambient temperature.20 The Zn-ion diffusion coefficient can be calculated using the following equation:
O.25 The peaks observed at 1403 cm−1 and 3136 cm−1 are attributed to the bending and stretching vibrations of the N–H bonds.27 The peaks at 1625 cm−1 and 3435 cm−1 indicate the stretching modes of crystal water present in NaNVOH and NaKNVOH. Additionally, a peak at 3010 cm−1 in NaKNVOH suggests the formation of hydrogen bonds (N–H⋯O) with some covalent character between the [VOn] and NH4+ layers, which contributes to the stability of the layered structure.28 Upon careful inspection, NaKNVOH exhibits a redshift of 3.7 cm−1 for the H–O–H bending mode and 2 cm−1 for the N–H stretching mode, which is related to the modified interaction between H2O and NH4+.29 In the Raman spectra (Fig. 1c), the peaks at 285 and 994 cm−1 are attributed to the bending and stretching vibration modes of the V
O double bond.30 The peaks at 193 and 694 cm−1 represent the stretching vibration of V–O bonds. The peak at 408 cm−1 corresponds to the stretching vibration of the V2–O bonds.31 The peak at 140 cm−1 is associated with the bending vibration of the –V–O–V–O– chains, indicating a long-range ordered structure related to the layered configuration.32 To verify the effects of single Na+ intercalation or co-insertion of K+ and Na+, thermogravimetric (TG) and electron paramagnetic resonance (EPR) analyses were performed. The TG curves for NaNVOH and NaKNVOH are presented in Fig. 1d. The initial weight loss corresponds to the desorption of physically adsorbed water. The subsequent weight loss represents the release of crystal water and ammonium ions. The final stage involves the complete removal of ammonium ions accompanied by a crystallization process. Notably, the total mass losses corresponding to NH4+ and crystalline water were measured as 7.68% and 5.97% for NaNVOH and NaKNVOH, respectively. Both samples exhibit an EPR signal with a g value of 2.0, indicating the presence of V4+ ions (Fig. 1e).33,34 The vibration in intensity is due to the different proportion of V4+ and oxygen vacancies. The higher signal intensity observed in NaNVOH suggests a higher ratio of V4+ ions and oxygen vacancies. This phenomenon arises because the sole incorporation of Na+ into the [VOn] layers induces localized charge imbalance. To maintain electro neutrality, the system compensates for the positive charge deficiency through oxygen vacancy formation (via O2− elimination). The synergistic incorporation of K+ and Na+ achieves balanced charge compensation across distinct lattice sites, significantly reducing the reliance on oxygen vacancy generation.35 The contents of K, Na, V, and N in both samples were quantified by inductively coupled plasma optical emission spectrometry (ICP-OES) analysis and an oxygen/nitrogen/hydrogen analyzer (ONH), as depicted in Table S1. The chemical formulas of NaNVOH and NaKNVOH were determined to be Na0.10(NH4)1.04V4O10−y·0.52H2O and K0.16Na0.05(NH4)0.71V4O10−x·0.63H2O, respectively.
The chemical states of NaNVOH and NaKNVOH were further investigated by X-ray photoelectron spectroscopy (XPS) (comprehensive XPS spectra in Fig. S1). In the V 2p spectrum (Fig. 1f), the co-doping of K+ and Na+ increases the proportion of V4+ from 11.30% to 30.15%. It demonstrates that the charge compensation mechanism for K+ and Na+ involves the reduction of some vanadium ions (V5+) to the lower valence state (V4+) for maintaining charge neutrality.36 In the O 1s spectra (Fig. 1g), the binding energies of 531.55 eV, 529.90 eV, and 528.84 eV are attributed to absorbed H2O, oxygen vacancies (Ov), and lattice oxygen, respectively. High-resolution K 2p (Fig. 1h) and Na 1s (Fig. S2a) spectra confirm the co-intercalation of K+ and Na+ in NaKNVOH, while only Na+ is inserted in NaNVOH. Additionally, the broadening of the Na 1s peak in NaKNVOH is attributed to the different sodium environment.37 In the N 1s spectra (Fig. S2b), the signal corresponds to –NH– (398.26 eV) and –N+H– (400.14 eV). Furthermore, the shift of the V 2p peak towards lower binding energy and the shifting of the O 1s and N 1s peaks to higher binding energies after dual-ion doping further demonstrate that it induces a secondary electronic rearrangement in the local chemical environment.
Scanning electron microscopy (SEM) and transmission electron microscopy (TEM) images of NaKNVOH (Fig. S2a and b) show that it grows uniformly on titanium foil, forming nanowire arrays. In addition, the morphology of NaKNVOH is similar to that of NaNVOH (Fig. S3a and b), indicating that the incorporation of K+ does not change the morphology. EDS mapping in Fig. 2c demonstrates that the K, Na, N, V, and O elements are uniformly distributed throughout the entire nanobelt, while NaNVOH only shows Na, N, V, and O elements (Fig. S3c), further confirming the controllable introduction of alkali metal ions. The high-resolution TEM (HRTEM) images of NaNVOH (Fig. 2d) exhibit lattice spacings of 2.97 Å and 1.77 Å corresponding to the (112) and (−603) planes in the [1–52] zone axis, as confirmed by fast Fourier transform (FFT) and inverse fast Fourier transform (IFFT) analyses (Fig. 2f). The HRTEM images of NaKNVOH (Fig. 2e) show lattice spacings of 3.23 Å and 1.82 Å along the [−101] zone axis for the (111) and (020) planes (Fig. 2g). Additionally, geometric phase analysis (GPA) was used to assess the strain distributions.38 Compared with NaNVOH (Fig. 2e), the strain distribution of NaKNVOH (Fig. 2f) along the xy axis is more homogeneous with the intercalation of Na+–K+-in-subsequenced, which can mitigate structural collapse caused by localized lattice distortions.39
The advantages of the “Na+–K+-in-subsequence” strategy in the material are clarified through a comparative assessment of the rate performance and cycling stability of NaNVOH//Zn and NaKNVOH//Zn batteries. The NaKNVOH cathodes exhibit specific capacities (Fig. 3c) of 495.4, 414.2, 327.1, 230.6, and 177.8 mAh g−1 at current densities of 0.25, 0.5, 1.0, 2.5, and 4.0 A g−1, as determined from GCD profiles depicted in Fig. 3d. When the current densities are reverted to 2.5, 1.0, 0.5, and 0.25 A g−1, the discharge capacities recover to 208.4, 298.4, 372.6, and 451.3 mAh g−1. NaKNVOH//Zn demonstrates a superior rate capability with higher specific capacities compared to NaNVOH//Zn (Fig. 3c and S4) at equivalent current densities. After returning to the initial current density, the capacity retention rate of NaKNVOH is 91%, while that of NaNVOH is only 79%, highlighting the robust tolerance of NaKNVOH to rapid Zn2+ (de)intercalation. Fig. 3f shows the cycling performance of the two cells at a low current density of 0.5 A g−1. The initial specific capacity of the NaKNVOH cathode is 336.03 mAh g−1, and after 300 cycles, it retains a specific capacity of 316.69 mAh g−1, corresponding to a capacity retention rate of 94.2%. This is significantly higher than the capacity retention rate of the NaNVOH//Zn battery, which is 64% with an initial specific capacity of 300.92 mAh g−1. The GCD curves of NaKNVOH are shown in Fig. S5a, with a gradient from pink to blue visually demonstrating this stability compared to NaNVOH (Fig. S5b). The long-term cycling performance of the two electrodes was further tested at a high current density of 4.0 A g−1. As shown in Fig. 3g, the NaKNVOH cathode exhibits an initial discharge capacity of 193.30 mAh g−1, which gradually increases to 208.86 mAh g−1 after 230 cycles. This increase can be attributed to infiltration and electrochemical activation processes,42,43 a phenomenon also observed in previous studies on layered vanadate and manganite.44,45 Subsequently, the capacity stabilizes at 186.67 mAh g−1 after 2000 cycles, yielding a high capacity retention rate of 96.57% with a coulombic efficiency (CE) close to 100%. However, the fluctuations during cycling are due to changes in ambient temperature.20 SEM images of the NaKNVOH cathode in its initial state and after 2000 cycles (Fig. 3g1 and g2 ) confirm that the nanowire morphology remains well-preserved. Additionally, the XRD pattern of NaKNVOH after 2000 cycles (Fig. S6) shows almost no byproducts. In contrast, NaNVOH electrode exhibits rapid capacity decay after initial fluctuations, starting from 192.32 mAh g−1, with only 72.23% capacity retention after 1000 cycles. Fig. S8 and Fig. 3h present the dQ/dV analysis of NaNVOH and NaKNVOH cathodes after 2000 cycles at 4 A g−1. At high current densities, both cathodes exhibit two distinct peaks: an oxidation peak (O1) at ∼1.3 V (V5+) and a reduction peak (R1) at ∼0.6 V (V3+). As the number of cycles increases, O1 shifts to a higher voltage and R1 shifts to a lower voltage due to polarization. The intensity of O1 gradually increases, with NaKNVOH showing a higher dQ/dV peak than NaNVOH. This suggests that the gradual activation of NaKNVOH results in more active sites, enhancing the reaction rate. The observed fluctuating capacity can be attributed to variations in the diffusion-controlled contribution, which are influenced by changes in interlayer spacing and environmental temperature, ultimately leading to capacity fluctuations.45 In addition, to further present the superiority of NaKNVOH//Zn battery, their performances were compared with those of the previously reported ammonium vanadate (Fig. 3e), including (NH4)2V10O25·8H2O and NVO. NaNVOH cathode possesses better comprehensive performance.46,47
The charge storage mechanisms of NaKNVOH//Zn and NaNVOH//Zn batteries are investigated through comprehensive electrochemical kinetic analysis. As illustrated in Fig. 4a, the cyclic voltammetry (CV) scanning rate is increased from 0.2 mV s−1 to 1.0 mV s−1. The observed slight peak shift is attributed to polarization effects during Zn2+ (de)intercalation processes. Furthermore, the well-shaped V4+/V3+peak (pointed out by the black arrow) of NaKNVOH also verifies that the Na+–K+-in-subsequence effectively facilitates the multivalent redox transitions of V5+/V4+/V3+, thereby reducing the potential gap between oxidation and reduction and improving the reversible transformation of the [VOn] layer.48–50 The relationship between the peak current (i) and scan rate (v) is described by the power-law equation:51,52
| i = avb | (1) |
The constants a and b represent the empirical parameters; the value of b is defined by the slopes of log(i) vs. log(v), as shown in the following equation:
| log(i) = b·log(v) + log(a) | (2) |
In general, the value of b ranges from 0.5 to 1. A b-value of 0.5 suggests that the electrochemical behavior is solely governed by diffusion control, whereas a b-value of 1 indicates that the capacitive behavior is dominant. The b-value fitting curves for NaNVOH and NaKNVOH electrodes are presented in Fig. 4b. The b-values for the first and second peaks of NaKNVOH are 0.75 and 1.00, while both peaks of NaNVOH exhibit a b-value of 0.83. These results indicate that the charge storage mechanism of the cathode materials is primarily based on the combined action of pseudocapacitance and diffusion behavior. To further investigate the ratio in the total capacity, the pseudo-capacitive contribution ratio can be calculated by the formula:
| i = k1v + k2v½ | (3) |
The diffusion kinetics of Zn2+ in the lattice of NaNVOH and NaKNVOH during cycling is further studied via GITT measurements (Fig. 4d and e). The diffusion coefficient values of NaKNVOH (10−7.9–10−10.8) are higher than those of NaNVOH (10−8.3–10−11.4) during the entire discharging/charging process. It is worth noting that the sharp decline in the diffusion coefficient of NaKNVOH at the final point of discharge may be attributed to minor interfacial side reactions. In addition, as depicted in Fig. 4f, the diameter of the semicircle in the high-frequency region of the electrochemical impedance spectroscopy (EIS) plot is indicative of the charge transfer resistance (Rct). According to the fitting results of the equivalent circuit model, the Rct value for NaKNVOH electrode is determined to be 28.16 Ω, which is smaller than that of NaNVOH cathode, which has an Rct of 37.1 Ω.
The evolution of morphology and chemical states of the NaKNVOH cathode in different (dis)charging states is investigated via SEM-EDS mapping and XPS analysis. As shown in Fig. S10–S12, NaNVOH electrode exhibits partial fracture of its 3D architecture upon discharging, followed by structural collapse upon recharging to 1.6 V, whereas NaKNVOH maintains an intact 3D nanowire network throughout the entire discharge/charge process. As illustrated in Fig. 5c, the initial NaKNVOH cathode exhibits distinct Zn signals. Upon full discharge to 0.2 V, a significant enhancement in the Zn 2p peak intensity is observed, confirming more Zn2+ intercalation. When charged to 1.6 V, the Zn 2p peak intensity diminished, indicating the extraction of Zn2+ from the host structure. The V 2p spectra (Fig. 5d) reveal a decrease in the V5+ peak intensity, accompanied by the emergence of a V3+ peak upon discharge to 0.2 V, demonstrating a two-step reduction reaction from V5+ to V3+. Subsequent charging to 1.6 V restores the V5+ peak intensity while eliminating the V3+ signal, achieving near-identical spectral features to those of the pristine state. For the O 1s spectra (Fig. 5e), the intensity of the oxygen vacancy (Ov) peak decreases upon discharge to 0.2 V, concurrent with an increase in the H2O-related peak intensity. Moreover, the N 1s, K 2p, and Na 1s spectra (Fig. S13) verify that NH4+, K+, and Na+ exist stably during cycling. The reversible shift of the Na 1s peak to a lower binding energy during discharge and its recovery upon charging originates from the dynamic charge redistribution within the cathode framework. It suggests that the insertion/extraction of Zn2+ in NaKNVOH is reversible.
Density functional theory (DFT) calculations were conducted to clarify the impacts of K–Na dual ion and reveal the diffusion pathway and diffusion energy barriers of Zn2+ in NaNVOH and NaKNVOH. The geometrically optimized crystal structure is shown in Fig. 6a. The enlarged c-value of 10.64 Å compared to NaNVOH (10.51 Å) indicates that K+ intercalation weakens the compressive stress. The total density of states (DOS) (Fig. 6b) indicates that NaKNVOH displays a new electronic state and a lower conduction energy, suggesting optimized carrier migration efficiency, thus contributing to high capacity. Charge density difference analysis of NaNVOH and NaKNVOH (Fig. 6c) was performed to investigate the modulation of the electron structure. The negative charge distribution shifts toward the V atoms due to structural regulation, resulting in weaker electrostatic interactions between zinc ions and [VOn] layers during the zinc ion intercalation, thereby facilitating the diffusion kinetics. The top view of possible migration pathways for Zn2+ in NaNVOH and NaKNVOH is shown in Fig. 6e, where Zn2+ mainly diffuses along the b-axis as reported in similar studies.55 The energy barrier along the Zn2+ migration pathway for KNVO is approximately 0.55 eV in Fig. 6f, which is lower than that of NVO (∼2.39 eV), suggesting that Na+–K+-in-sequence optimizes the pathway and promotes faster Zn2+ migration.24
Supplementary information (Fig. S1–S13) is available. See DOI: https://doi.org/10.1039/d5dt01363a