Juyoung
Kim
a,
Satoru
Yamanaka
a,
Ichiro
Murayama
a,
Takanori
Katou
a,
Tomokazu
Sakamoto
a,
Takuro
Kawasaki
b,
Tatsuo
Fukuda
c,
Tohru
Sekino
d,
Tadachika
Nakayama
e,
Masatoshi
Takeda
e,
Masaaki
Baba
e,
Hirohisa
Tanaka
f,
Kazuya
Aizawa
b,
Hideki
Hashimoto
d and
Yoonho
Kim
*a
aAdvanced Research and Development Department, Daihatsu Motor Co., Ltd, 3000, Yamanoue, Ryuo, Gamo, Shiga 520-2593, Japan. E-mail: Yoonho_Kim@dk.daihatsu.co.jp; Fax: +81-74-857-1064; Tel: +81-74-857-1685
bJ-PARC Center, Japan Atomic Energy Agency, 2-4 Shirane Shirakata, Tokai, Naka, Ibaraki 319-1195, Japan
cMaterials Sciences Research Center, Japan Atomic Energy Agency, 1-1-1, Kouto, Sayo, Hyogo 679-5148, Japan
dThe Institute of Scientific and Industrial Research (ISIR), Osaka University, Mihogaoka 8-1, Osaka, Ibaraki 567-0047, Japan
eNagaoka University of Technology, 1603-1, Kamitomioka, Nagaoka, Niigata 940-2188, Japan
fKwansei Gakuin University, 2-1 Gakuen, Sanda, Hyogo 669-1337, Japan
First published on 24th December 2019
Waste heat is a potentially exploitable energy source but remains a problem awaiting a solution. To explore solutions for automobile applications, we investigate pyroelectric power generation from the temperature variation of exhaust gas using a novel electro-thermodynamic cycle. Niobium-doped lead zirconate titanate stannate (PNZST) ceramics were applied as pyroelectric materials, and their structural characteristics were investigated. In the driving cycle assessments (JC-08) using real exhaust gas, the maximum power generated was identified as 143.9 mW cm−3 (777.3 J L−1 per 1 cycle) over a temperature range of 150–220 °C and an electric field of 13 kV cm−1. The net mean generating power of the total driving cycle was 40.8 mW cm−3, which is the most enhanced result in our power generating systems to date and 314 times greater than our first report. Materials with sharp transition behaviors with the temperature and electric field are worthy of study with regard to pyroelectric energy harvesting materials, and their corresponding crystal and domain structures were investigated to optimize performance.
Pyroelectric materials that exhibit a PE have a polar symmetry in their crystal structure, leading to spontaneous polarization (PS). As the temperature increases, these materials undergo phase transitions from the ferroelectric phase to the paraelectric phase as PS changes. The decrease in polarization of the materials can be recovered as electrical work from the thermodynamic cycle. Perovskite structures such as Pb(Zr,Ti)O3 (PZT) and Pb(Mg1/3Nb2/3)O3–PbTiO3 (PMN–PT)-based ceramics have been utilized in many studies for energy harvesting due to their outstanding electrical properties. Pandya et al.8 reported that a maximum energy density and power density of 1.06 J cm−3 and 526 W cm−3, respectively, were scaled for ferroelectric PMN–PT thin films from the implementation of Ericsson cycles. Kim et al.1 reported the practical application of pyroelectric power generation using PZT-based ceramics for exhaust gas of an automobile by using a novel electro-thermodynamic cycle.
To improve the efficiency of power generation, the development of pyroelectric materials through diversified analysis is required. In this report, following previous studies,1,9–12 a practical assessment of the power generation performance was conducted using an engine dynamometer, for which we obtained considerably improved results with niobium-doped lead zirconate titanate stannate (Pb0.99Nb0.02(Zr0.637Sn0.273Ti0.09)0.98O3, PNSZT) ceramics. This material was characterized and investigated with respect to its phase structure and transition behavior in the cycles to discuss the proper direction of materials research in the pyroelectric power generation system.
PD = NDf |
STEP 1 (A–B): the external electric field (EH) is applied briefly to the sample when the temperature begins to increase, and the sample reaches maximum polarization.
STEP 2 (at point B): EH is removed by the diode when charging is completed.
STEP 3 (B–C1): in this period, we can obtain an additional voltage increase in the sample. The material is then isolated in the circuit (Fig. 1(c)), and the electric displacement D is kept constant while the temperature increases to TH. The internal electric field of the materials (dashed line) is increased along path BC1 based on the electro-thermodynamic equation dD/dt = εdE/dt − pdT/dt (where D, E, T, ε, t and p are the electric displacement, electric field, temperature, dielectric permittivity, time, and pyroelectric coefficient, respectively).
STEP 4 (C1–D): when the temperature begins to decrease, the switch is turned on and charged electricity immediately flows to R1 and R2. Finally, the material is reconnected to the circuit.
STEP 5 (D–A′): the D–E loop is closed by cooling back to TL and moving to point A. After the electricity has finished decreasing, the temperature continues to decrease when the switch is opened.
STEP 6 (at point A′): the switch is turned off before the next cycle.
Fig. 1(c) shows a harvesting circuit with a diode and two switches (DSW) redesigned based on the general Sawyer–Tower (ST) circuit to divide the input/output energy by the inductions of the diode and switch resistance (PP1 and PP2 for measuring the voltage of pyroelectric materials, and R1, R2 and RShunt for calculating the net generating power).
For power generation tests in the laboratory, a DSW circuit (Fig. 1(c)) was used as an energy-harvesting circuit.1,12 To simulate engine exhaust gas, two heat blowers (Hot Wind System, LEISTER) and a mechanical cylinder (ELCM4E10MK-AP, Oriental Motor) were employed. In the pseudosinusoidal temperature variation with a period of 0.05 Hz, the TH ranged from 100 to 200 °C with a temperature difference of ΔT = TH − TL = 40 °C, and the electric field was applied using a high-voltage amplifier (677B, TREK), synchronized to the pseudosinusoidal temperature variation.
A virtual vehicle simulator using an engine dynamometer based on exhaust gas (660cc, KF-VE3, Daihatsu Motor Co. Ltd.17) was used to evaluate the generating performance of the materials in a real environment, as shown in Fig. 2. The material was set into a special module case in the exhaust pipe with the circuit connected. The generating test was performed based on the Japanese fuel-economy and emission test driving cycle (JC08 mode).17,18
Fig. 2 A schematic diagram of the engine dynamometer assessment (Daihatsu, home-made). The pyroelectric material is set inside the generating module (main muffler). |
Atom | x | y | z | B |
---|---|---|---|---|
Pb | 0.23281(5) | 0.23281(5) | 0.23281(5) | 1.414(11) |
Nb/Zr/Sn/Ti | 0 | 0 | 0 | 0.280(14) |
O | 0.28287(11) | 0.22625(12) | 0.77480(14) | 2.053(17) |
Fig. 3(b) presents the microstructure obtained from TEM observations. The anisotropic domains were less than 50 nm thick and had hierarchical lamellar-like structures. The high density of nanoscale domains occurred due to small domain wall energies, which could facilitate the reorientation of polarization.20In situ experiments were performed along the individual cycle points A, B, C1 and D in Fig. 1(b). According to the TH and EH variations, the reversible response to the temperature and external electric field of the domains was confirmed.
Fig. 4(a) shows the temperature dependence of D–E hysteresis loops for the ceramics. The spontaneous polarization (Ps) and remnant polarization (Pr) respectively reached 34.32 and 29.79 μC cm−2 and the coercive field (Ec) reached 7.63 kV cm−1 at room temperature, indicating square loops typical of a ferroelectric (FE) state. The Ps, Pr and Ec decreased with temperature, and the antiferroelectric (AFE) region could be found shortly with double loop hysteresis in the vicinity of 150 °C before slim loops of a paraelectric state (PE) appeared. When an electric field above 5 kV cm−1 is applied while the temperature increases, the materials have a FE–PE phase transformation according to the temperature without going through the AFE phase. Berlincourt et al.21 confirmed the phase diagram of Pb0.99Nb0.02(Zr0.73Sn0.27Ti0.07)0.98O3 ceramics with the electric field and demonstrated that the incipient AFE state acts to increase the slope of the FE–PE boundary. As shown in Fig. 4(b), the polarizations of PNZST ceramics as a function of temperature decrease sharply while undergoing phase transformation corresponding to the D–E loop results. The sharp polarization behavior of PNZST compared to that in our previous study (C-6, PZT-based ceramics)1 can be expected due to the atomic ordering in the lattice22,23 and phase state under cycles.24,25 A rhombohedral phase has more available orientations for polarizations than a tetragonal phase such as the C-6 sample, leading to a naturally softer domain reorientation. This means that the rhombohedral state is relatively liable to rotate polarization with a small Ec and can maximize the energy generation by reducing the input energy.
Fig. 4 (a) Hysteresis D–E loops and (b) the polarizations of the PNZST ceramic as a function of temperature. |
The generating performance was evaluated using the DSW circuit in Fig. 1(c). The temperature variation ΔT (=TH − TL) was set to be 40 °C considering the average temperature variation of the practical mode environment, and EH reached up to 12 kV cm−1 under each temperature condition. Fig. 5(a) presents the net mean power (Pnet) generated by PNZST samples according to TH and E. The peak of Pnet was obtained when the TH was near 180 °C (temperature range between 140 °C and 180 °C), including the FE–PE transition region in which the largest change in polarization occurred due to depolarization of the material above the transition temperature.26 As higher EH was applied, the Pnet increased and the temperature of the Pnet peak became higher. This indicates that the temperature of the FE–PE transition increase was a function of EH.21 The maximum Pnet observed was 11 mW cm−3 (generating energy of 220 J L−1 per 1 cycle) at TH = 190 °C (temperature range between 150 °C and 190 °C), which is a significantly enhanced value compared to the PZT-based ceramics in our previous study (C-9: 0.16 mW cm−1). Above TH = 190 °C, the change in polarization decreased, which resulted in the degradation of Pnet.
Fig. 5(b) shows the measured D–E behavior of PNZST samples undergoing the generating cycle (at TH = 180 °C and EH = 12 kV cm−1), which is calculated from the charge of the connected capacitor. Compared to the theoretical area of the isothermal D–E loop, there are gaps in electrical displacements which are mainly due to cycling conditions. As shown in Fig. 1(b), when the EH applied in the A–B process, the temperature of the material already increases, which makes a difference with regard to its theoretical isothermal behavior. The process C1–D also has losses because the material is undergoing the cooling step during the recovery of the energies. On the other hand, at point D, the polarization of the material vanishes above the FE–PE transformation temperature and a certain level of electric field is needed to realign the dipoles until the full repolarization of point B. Materials that are liable to rotate polarization have high slopes of the A–B route linked with their high power generating potential.
An engine dynamometer assessment using real exhaust gas was conducted based on the Japanese fuel-economy and emission test driving cycle (JC08 mode), as shown in Fig. 2. In the redesigned main muffler, the temperature of the exhaust gas was controlled to include the phase transition region of the PNZST samples, and the external EH was optimized as 13 kV cm−1 for each representative temperature variation (Fig. 6(a) and (b)). Fig. 6(c) shows the individual calculated energy densities of each temperature variation in the mode. The maximum generating power was 143.9 mW cm−3 (generating energy of 777.3 J L−1 per 1 cycle) in the temperature range of 150–220 °C and the detailed cycle behavior is shown in Fig. 7. In this cycle, the speed condition of the vehicle is the range of about 0–40 km h−1 and the acceleration is about 10 m s−2. Fig. 6(d) presents the results of the assessments over the total drive cycle with PNZST samples compared to previous results.1,9 The net mean power was 40.8 mW cm−3 (accumulated generating energy of 49117.4 J L−1), which is the highest value produced by any material in our energy harvesting system to date1,9–12 and is 314 times greater than what we presented in our first report.1
Fig. 7 The maximum generating power cycle in the test and its conditions: TL = 150 °C, TH = 220 °C, and EH = 13 kV cm−1. |
The comparisons of the current maximum power and energy density for pyroelectric energy harvesting studies for various materials are shown in Table 2, together with the respective operating conditions. PNZST ceramics in this study have a sharp phase transition behavior with the temperature from the rhombohedral phase with many axes of polarization (the number of available orientations for the polarization in the lattice is eight in the rhombohedral phase and six in the tetragonal phase for pervious samples), and the polarization rotates easily with the external electric field with a small Ec, such that enhanced power generating was obtained. These materials have enormous potential for high performance and can be advantageously utilized for many other device applications in addition to this automobile system. According to the practical system environment of devices, the generating power can be enhanced more by thinning the samples, controlling the temperature and frequency, and improving the breakdown voltage.
Material | Temperature TH/TL (°C) | Electric field EH/EL (kV cm−1) | Frequency of the experimental cycle (Hz) | Energy density (J per L per cycle) | Power density (mW cm−3) | Ref. |
---|---|---|---|---|---|---|
PNZST ceramics | 220/150 | 13/0 | 0.185 | 777.3 | 143.9 | This study |
PZN-4.5 PT single crystals | 160/100 | 20/0 | 0.1 | 217 | 21.7 | 27 |
PMN-10PT ceramics | 80/30 | 35/0 | — | 186 | — | 28 |
PMN-32PT thin films | ΔT = 56 | ΔE = 267 | 1000 | 526 | 526000 | 8 |
PNZST ceramics | 177/157 | 32/4 | 0.26 | 131 | 34 | 29 |
PLZT ceramics | 160/25 | 75/2 | 0.0178 | 888 | 15.8 | 30 |
PNNZT ceramics | 220/20 | 90/3 | 0.09 | 867 | 78 | 5 |
P(VDF-TrFE) thin films | 110/25 | 500/200 | 0.13 | 441 | 58 | 31 |
BCT-BZT-Fe ceramics | 110/30 | 30/0 | Calculated from the D–E diagram | 305 | — | 32 |
BNK-BST ceramics | 160/20 | 40/1 | 1523 | — | 33 | |
BNKT ceramics | 110/25 | 52/1 | 1986 | — | 34 | |
PZT/CFO-L3 thin films | 27/−173 | 400/0 | 47372 | — | 35 |
We consider that the high performance materials used for pyroelectric energy harvesting mostly have an appreciable change in polarization behavior in each cycle, as well as a corresponding crystal structure. In addition to this, we speculate that materials that are composed of nanoscale anisotropic domains and have many axes of rotatable dipoles have higher performance. An investigation of the structural changes in pyroelectric materials in terms of the crystal and domain scale is presented herein, and future research regarding energy harvesting will continue to address these characteristics for the design of high performance materials.
This journal is © The Royal Society of Chemistry 2020 |