Ashour M. Ahmed*a,
Mohamed Rabiaab and
Mohamed Shabana
aNanophotonics and Applications (NPA) Lab, Physics Department, Faculty of Science, Beni-Suef University, Salah Salem Street, Beni-Suef, 62514, Egypt. E-mail: ashour.elshemey@gmail.com; ashour.mohamed@science.bsu.edu.eg
bPolymer Research Laboratory, Chemistry Department, Faculty of Science, Beni-Suef University, Beni-Suef, 62514, Egypt
First published on 9th April 2020
Nanocrystalline undoped and Cr-doped PbS thin films were prepared on glass substrates by a simple chemical bath deposition method. The X-ray diffraction analyses of the films showed their polycrystalline nature with cubic structure and preferential growth along the (111) orientation. Cr incorporation decreases the average PbS crystallite size from 59.97 to 37.59 nm, whereas the strain and dislocation density showed an increasing trend. The atomic ratio of doping for Cr is about 0.63, 1.75, and 4.70% according to energy-dispersive X-ray (EDX) spectroscopy. Morphological analysis showed that the average sizes of nanoclusters decreased from 73 to 41 nm as the Cr concentration increased. The optical band gap values are increased with increasing Cr doping. The photoelectrochemical (PEC) behaviors and the stability of the Cr doped PbS photoelectrodes were studied in 0.3 M Na2SO3 electrolyte solution. Also, the incident photon-to-current efficiency and applied bias photon-to-current efficiency are calculated and showed optimized values of 13.5% and 1.44% at 0.68 V and 390 nm. Moreover, the optimized electrode shows high chemical stability and a long lifetime. Finally, the effect of temperature on the PEC behaviors is evaluated and the different thermodynamic parameters are calculated.
PbS has the efficient light-absorbing capacity from the visible to near-infrared due to the bandgap of PbS can be tuned across visible to NIR region.10,11 Hence, PbS has good photocatalytic efficiency of hydrogen production.12 Also, the PbS nanoparticles can also show multiple exciton generations (MEG).13,14 In the MEG process, two electron–hole pairs (excitons) are produced by the absorption of one high-energy photon, bypassing hot-carrier cooling via phonon emission.15 This phenomenon was used to improve the photoconversion efficiency.16,17 Moreover, PbS possesses third-order nonlinear optical (3NLO) response 30 times that of GaAs and 1000 times that of CdS nanoparticles for particles of a similar size, which makes the PbS nanoparticles are suitable for optoelectronics applications.6,18
Many authors have presented a great interest in the study of the doped PbS thin films with various metal elements19–21 to tuning their optoelectrical properties from the viewpoints of practical applications. The impurity atoms provide sharp atomic levels for capturing exciton electrons and holes from the host lattice which help in tuning the properties of PbS. The nature and concentration of the dopant are responsible for the improved physical properties and efficiencies of PbS based semiconductor devices.
Gulen reported manufacturing Fe-doped PbS films on glass substrates by the SILAR method. The optical bandgap of the PbS films decreased from 1.66 to 1.25 eV as the Fe-doping concentration is increased from 1 to 9% Fe-doped PbS.22 Touati et al. have detected a blue shift of the bandgap due to the quantum confinement effect for (0–8%) Ag-doped PbS thin films.23 A systematic decrease in the crystallite size with increasing Hg concentration in the PbS thin films was reported by Palomino-Merino et al.24 Also, Portillo et al. showed that wide bandgap could be obtained for PbS nanocrystals doped in situ simultaneously with Er–Cd–Bi.25 In addition, the optical absorption of Mn, Cd and co-doped PbS nanocrystals have been investigated by Saravanan et al.26
Most of the previous work focused on enhancing the PEC properties by deposited PbS nanoparticles on different photoelectrodes such as ZnO, TiO2, and CuO–Fe2O3. Hsu et al. studied Al-doped ZnO nanorod thin film decorated with PbS nanoparticles as a photoelectrode for solar water splitting.16 The enhancement in the photocurrent density is due to the lowering of energy bandgap. Zhao et al. introduced a green synthesize of near-infrared PbS/CdS core/shell quantum dots on TiO2 mesoporous photoanode for photocatalytic hydrogen production.27 Shi et al. studied the multiple exciton generations using ZnO@PbS/graphene oxide photocatalyst for H2 production from water. The H2 evolution efficiency is remarkably improved by the synergistic effect of multiple exciton generations combined with the electron–hole separation of graphene oxide.28
Although the previous attempts, there are substantial needs for low cost, stable, and more efficient photoelectrochemical electrodes toward the industrial hydrogen production. However, less work was devoted to the photoelectrochemical properties based on PbS thin films.
On the other hand, chromium (Cr) is a typical transition metal element with a relatively abundant in the earth's crust. This element can be used in many applications such as dyes, paints, stainless steel alloys, a protective layer, blast furnaces, artificial rubies, catalysts for processing hydrocarbons, and recording magnetic tapes due to its physicochemical properties. The Cr can enhance the interaction with light because it possesses surface plasmon interactions.29 Also, chromium metal crystallizes as a body-centered cubic lattice with a lower energy of the high spin configuration. In addition, it has abundant electrons in the outer shell of its electronic configuration. Hence, it exhibits several oxidation states, ranging from −4 to +6.
In a previous literature report, the oxidation state of Cr ion in the Cr-doped PbS sample is +3 (ref. 30). The +3 state is a common oxidation state of Cr due to it is the most stable energetically according to crystal field theory (CFT).31,32
The Cr3+ has an ionic radius very small compared to that of the Pb2+ ion. The electronegativity of Cr (1.66) is lower than that of Pb (2.33) on the Pauling scale. Hence, incorporation of Cr3+ ions into the host PbS lattice permits more dopant ions to be accommodated in the Pb2+ sites thereby influence its physical properties. In many previous studies, the photoelectrochemical activity of photoelectrodes such as TiO2 and Fe2O3 show significant enhancement by doping with Cr due to an improvement in charge carrier properties.33 To the best of our knowledge, the photoelectrochemical studies on the Cr-doped PbS thin films have not been reported in the literature.
In the present work, Cr was chosen as a dopant for PbS thin films. Cr-doped PbS thin films with different concentrations of Cr were prepared by chemical bath deposition (CBD) method. The CBD is simple, low cost, good quality material and uniform coating at low temperature. The effect of Cr doping on the morphological, structural and optical properties of PbS thin films was investigated, and the results are presented. Also, the photoelectrochemical behaviors of the Cr-doped PbS films for the generation of H2 under visible irradiations are addressed.
For the deposition of PbS thin films, lead nitrate Pb(NO3)2 and thiourea CS(NH2)2 were used as the source of cationic Pb2+ and anionic S2− precursor solutions, respectively. Sodium hydroxide NaOH was used as the complexing agent, which helps to control the reaction rate and prevent the formation of hydroxide precipitates. All the chemicals were analytically pure, and all aqueous solutions were prepared using DI water.
In a typical reaction, the bath solution was prepared by the sequential addition of 90 ml (10 mM) of lead nitrate and 90 ml (57 mM) of thiourea mixed with 90 ml (146 mM) of sodium hydroxide. These molar ratios are optimized after many experimental trials using varied ratios to obtain homogenous films with high uniformity and adhesion. It is worth to mention that not all thiourea are simultaneously decomposed to give S atom, so the molar ratio of thiourea is higher than the molar ratio of the lead nitrate. The solutions mixed in this order to obtain a final dark solution, a change may provide a different product at the end. The solution was stirred for 2 minutes to get a homogeneous solution. The final pH of the mixture was measured to be 12.8. The cleaned glass was vertically immersed in bath solution for 30 min at room temperature without stirring. In the beginning, the deposition bath was colorless, and its color has changed from brown to dark grey with time deposition.
The following eqn (1)–(5) give the reaction process for forming PbS film.34
Pb(NO3)3 + 2NaOH → Pb(OH)2 + 2NaNO3 | (1) |
Pb(OH)2 + 4NaOH → Na4Pb(OH)6 | (2) |
Na4Pb(OH)6 → 4Na + HPbO2− + 3OH− + H2O | (3) |
SC(NH2)2 + OH− → CH2N2 + H2O + SH− | (4) |
HPbO2− + SH− → PbS + 2OH− | (5) |
After deposition, the films were cleaned by rinsing with distilled water and then dried in air. Mirror-like thin film surface was obtained after removal of the deposited film from one side of the glass slide using cotton with dilute H2SO4. Finally, the films were annealed in air at 250 °C in a furnace for 2 h to improve the crystallinity of the films. The annealed films appear to be smooth, homogeneous and well adherent to the glass substrates.
Fig. 1 (A–C) XRD spectra for nanostructure pure and doped PbS thin films with different Cr content. (D) The lattice parameter for (111) and (200) planes. |
There exist three variants to include Cr atoms in PbS nanoparticles. First, Cr can substantially replace Pb. Second, Cr atoms can occupy interstitial positions. Third, Cr atoms can take their places between the layers of PbS (intercalation) or take place on the internal and external surfaces of nanoparticles.
No additional XRD peaks were observed for Cr metal or Cr oxide due to the low amount of Cr-loading, which is below the detection limit of XRD.
The Cr doping did not significantly change the phase structure of the PbS crystal but the neighboring atoms of the Cr atom remain under tensile stress because the substantial Cr3+ ions (RCr3+ = 0.615 Å) are smaller in size compared to the original Pb2+ ions (RPb2+ = 1.19 Å). Similar results were obtained by Kayani et al. for ZnO thin films doped with Cr and prepared by sol–gel dip-coating method.35
Moreover, the structural XRD parameters for the highest four peaks; (111), (200), (220) and (311); are calculated and mentioned in Table 1. The crystallite size (D), lattice parameter (a), texture coefficient (TC), interplanar distance (d), strain (ε), and dislocation constant (δ) are calculated by using the following equations;36,37
D = 0.94λ/βcosθ | (6) |
(7) |
d = λ/2sinθ | (8) |
(9) |
ε = 0.25βcotθ | (10) |
δ = D−2 | (11) |
Film | hkl | TC | D (nm) | d (Å) | a (Å) | ε × 10−2 | δ ×10−4 (nm−2) |
---|---|---|---|---|---|---|---|
PbS (pure) | (111) | 2.6 | 63.873 | 3.441 | 5.960 | 26.937 | 2.4510 |
(200) | 2.0 | 64.390 | 2.979 | 5.959 | 23.137 | 2.4118 | |
(220) | 1.1 | 51.672 | 2.104 | 5.951 | 20.359 | 3.7452 | |
(311) | 0.51 | 32.172 | 1.792 | 5.946 | 27.863 | 9.6610 | |
PbS-Cr2 | (111) | 2.17 | 63.870 | 3.444 | 5.966 | 26.964 | 2.4512 |
(200) | 1.67 | 49.793 | 2.973 | 5.947 | 29.859 | 4.0331 | |
(220) | 0.77 | 31.212 | 2.101 | 5.943 | 33.663 | 10.264 | |
(311) | 0.18 | 21.189 | 1.795 | 5.953 | 42.356 | 22.271 | |
PbS-Cr4 | (111) | 1.93 | 63.855 | 3.462 | 5.995 | 27.114 | 2.4524 |
(200) | 1.14 | 30.055 | 2.989 | 5.979 | 49.739 | 11.070 | |
(220) | 0.57 | 31.192 | 2.110 | 5.967 | 33.822 | 10.277 | |
(311) | 0.34 | 43.606 | 1.798 | 5.964 | 20.624 | 5.2590 | |
PbS-Cr6 | (111) | 1.70 | 40.422 | 3.434 | 5.947 | 42.476 | 6.1199 |
(200) | 1.31 | 30.062 | 2.979 | 5.959 | 49.556 | 11.064 | |
(220) | 0.56 | 42.312 | 2.104 | 5.952 | 24.868 | 5.5855 | |
(311) | 0.40 | 43.637 | 1.792 | 5.946 | 20.542 | 5.2515 |
From the calculation data, the average crystal size (D) for the planes (111), (200), (220) and (311) of the pure PbS is found to be 53.026 nm and decreases to 39.108 nm with increasing Cr doping ratio to 6.0 ml due to the diffraction peak broadening of PbS thin films and induced strain. The peak broadening can result from an increase in heterogeneity of the films due to the occupation of Cr3+ into the host lattice.24 The crystallite and grain sizes play an important role in the optical properties of the films. The peak intensity of XRD depends strongly on the Cr percentage, which decreases with an increase in Cr concentration. For the main peak (111), the diffraction intensity peak decreased from 159.82 to 56.31 acts as a concentration increase from 0 to 6 ml.
The texture coefficient (TC) was evaluated to quantify the preferred crystallographic orientations of the samples. It was observed from Table 1 that the plane (111) has a high texture coefficient, indicating that the nanocrystals have preferential coordination towards the (111). In many previous works, the (200) preferential growth was observed for PbS thin films.34,38 The variation of preferred orientation can be explained from the thermodynamic point of view. Xigui et al. have proposed that the reason for this variation is the change of the total system free energy during the film growth which is affected by the surface, interface and strain energy contributions.39 Moreover, the degree of these three energies contributions may be different under certain preparation conditions, which consequently leads to different preferred orientations.40
For all planes, increasing Cr ions content is associated with a decrease of the TC, as shown in Table 1, as a result of a decline in the crystal quality. The values of TC for (111) plane are decreased from 2.6 to 1.70 as the Cr volume content increased from 0 to 6 ml. The decrease of TC values reveals to the reduction of the film crystallinity. Hence, the crystal quality deteriorates with increasing Cr concentration. Previously, Haazen observed that the crystal quality of the insulator Bi2Se3 weakens with increasing Cr concentration.41
In the case of pure PbS film, main peaks are assigned to (111), (200), (220), (311) planes at 2θ = 25.89°, 29.98°, 42.98°, and 50.93° respectively. Also, the presence of the other peaks such as (222), (331), and (420) was identified with lower intensities. The number of diffraction peaks is decreased from 7 to 4 peaks with increasing of the Cr percent from 0 to 6 ml in the PbS films. So, the increase of Cr concentration in the precursor suppressed the crystal growth of the PbS in the (222), (331) and (420) directions. The Cr ions may have terminal OH− ligands in solution. Therefore, increased Cr concentration affects the concentration of OH− ions that are consumed for thiourea (TU) decomposition and subsequent release of free S2− ions.
The peak position of planes (111) and (311) are moved towards lower angles with increasing of the Cr percent in the films from 0 to 4 ml, but after that, the position moved towards higher angles. This shift can be attributed to doping-induced structural lattice deformation and disorder in the PbS crystal. Lattice constant changes are closely correlated to the shifts of the 2theta positions of XRD peaks. As a result of the increase of the lattice, the diffraction peaks are shifted towards lower Bragg angles. The changes of the lattice constant can be explained through three doping-sensitive factors: size effect, electronic deformation of the consistent conduction band minimum, and (iii) doping-induced variations of the lattice vibration anharmonicity. The distribution of Cr3+ in PbS lattice changes with increasing Cr concentration. Cr-doped PbS films with low Cr concentration could reach equilibrium. Accordingly, the low Cr concentration to a certain degree disorder the crystal lattice relative to the pure PbS lattice. Hence, the lattice constant increased and the diffraction angle decreased. By increasing the Cr% the distribution of the Cr3+ improved. Since the radius of the substantial Cr3+ ion is smaller than the radius of the original Pb2+ ion. Then, a larger Cr doping (>4%) should decrease the lattice constant (Table 1) due to the tensile stress on the neighboring atoms and structural relaxation. As a result, the diffraction angle is increased.
The interplanar distance (d) and lattice parameter (a) are increasing with increasing the Cr percent in the films from 0 to 4 ml but after that it with Cr percent. These due to the angle of diffraction θ is inversely related to the interplanar spacing d (sinθ is proportional to 1/d) according to Bragg's law.
The increase in the lattice parameter is not expected because the ionic radius of Cr3+ (0.63 Å) is smaller than that of Pb2+ ions (1.01 Å). In Cu-doped Bi2Se3, the copper (with an ionic radius of 0.71 Å) is substituting the bismuth (with an ionic radius of 1.17 Å) in the lattice and located between quintuple layers inside the van der Waals gap of the crystal structure.41 A similar mechanism is introduced to explain the increase of the lattice parameters (a) in the Cr-doped films.
The obtained lattice parameter ‘a’ values in Table 1 are found to be slightly higher than the standard value (5.9362 Å) due to the presence of intrinsic defects and loss of stoichiometry of the synthesized PbS-Cr films.
The lattice parameter ‘a’ has a nonlinear relationship with the content of Cr3+ for (111) and (200) planes, which not follow Vegard's law (Fig. 1(D)). This result demonstrates that the Cr ions are incorporated nonhomogeneous into the host PbS matrix due to the difference in the ionic radius and chemical oxidation states.
Increasing in lattice parameter with an increase in Cr3+ percentage produces expansion in the PbS unit cell. Therefore, the high strain is induced in crystal, and hence, crystalline qualities are deteriorated. The origin of strain is related to lattice misfit which in turn depends upon the growing conditions of the films.42 The strain increased from 0.2457 for pure PbS to 0.3436 for PbS-Cr6.
Dislocations are imperfections in a crystal that associated with misregister of the lattice in one part concerning another part of the crystal. The dislocation density (δ) defined as the length of dislocation lines per unit volume of the crystal. The value of δ for Cr-doping PbS films is higher than that of pure PbS film, which supports the increment in the number of defects in the doped PbS films. The increase in dislocation density suggests that films become less crystalline.43 Therefore, the presence of dislocations strongly influences many properties of the prepared materials.
The chemical compositions of the PbS and PbS-Cr films were studied by energy-dispersive X-ray (EDX) spectrometry. Fig. 2 shows the EDX spectrum of the PbS-6Cr film. The quantitative analysis of the PbS and PbS-Cr films are shown in Table 2. The EDX patterns indicated the presence of Pb, S and Cr signals as the components of the synthetic thin films as seen in Fig. 2 and Table 2. No impurities are detected in the EDX patterns, which indicate the films are well-crystallized and they are in good agreement with the XRD results. The ratio of Cr in the PbS-Cr films increased from 0 to 4.70% as the volume of CrO3 added to the PbS bath increasing from 0 to 6 ml. The atomic ratio of Pb:S:Cr is 42.92:52.39:4.70 for the PbS-Cr6 film.
Film | Element | ||
---|---|---|---|
Pb atomic% | S atomic% | Cr atomic% | |
PbS | 44.43 | 55.57 | 0 |
PbS-Cr2 | 46.11 | 53.26 | 0.63 |
PbS-Cr4 | 43.01 | 55.24 | 1.75 |
PbS-Cr6 | 42.92 | 52.39 | 4.70 |
Fig. 3 SEM micrographs for (A) pure PbS, (B) PbS-Cr2, (C) PbS-Cr4 and (D) PbS-Cr6 thin films. The lower insets of (A) and (D) are cross-sectional SEM images. |
The doping with Cr was observed to modify the surface morphologies and grain sizes, Fig. 3(B–D). It is clear that the surfaces of Cr-doped PbS films are formed from nucleation and coalescence of nanoparticles close to spherical granules with different diameters. The Cr-doped PbS nanoparticles are self-assembled to generate different voids with varied diameters.
As the Cr concentration increased, the average size of nanoparticles and the density of nanoparticles are decreased. The average size of nanoparticles decreases from 73 to 41 nm as the Cr volume content increased from 2 to 6 ml. This due to the Cr3+ ions consumes the OH− ions and hence reduces the growth rate. Therefore, the sizes of nanoparticles and the cluster of nanoparticles tend to be smaller and homogenize as the doping level increased. This means that the surface area of Cr-doped PbS films increases with increasing the doping level. The thicknesses of the films are increased from 320 nm for pure PbS to 450 nm for PbS-Cr6 as seen in the inset cross-sectional images of Fig. 3(A and D). Similar results were reported for Cr-doped CdO and Cr-doped ZnO thin films.44,45
All samples have two absorption bands; a sharp peak at UV region and a small broad one at the NIR region. These peaks attributed to band-gap absorption of PbS and structural defect absorption, respectively.46 The absorbance decreases sharply with wavelengths ranged from 300 nm up to 900 nm. The sharper peaks in the absorption spectra for all PbS films indicate a narrow size distribution of the nanoparticles. These spectra show an abrupt change in the doped samples compared to pure PbS. As seen in Fig. 4(A), the absorbance is decreased by increasing the Cr doping concentration. This is accompanied by a color change of PbS films from dark grey to red-grey with increasing Cr ratio. Jiabin Huo et al. observed similar behavior for Cr-doped PbS nanofilms.30 The absorption edge gradually shifted from longer wavelengths (near IR region) to shorter wavelengths (visible region) in the doped films signifying an increase in their bandgap values. These shifts are due to the decrease in the crystallite size as a result of the confinement effect. A clear absorption edge shown by all the grown thin films confirms the crystalline nature of the material.
From Fig. 4(B), the general behavior of transmittance spectra can be divided into three regions. At low wavelength in the UV region, all the PbS thin film having a nearly zero transmittance, which is due to strong absorbance in this region. In the medial part of spectra (550–1000 nm), the transmittance of the films varies linearly with wavelength. In the NIR region, a slight decrease in transmittance consequently for high wavelength electronic transitions are existing in this wavelength range. It can be seen that PbS film has a transparency of about 30% in the near IR region of the spectrum. Touati et al. obtained the same behavior for PbS thin doped with Cu metal.47
The film's transparency of pure PbS below 900 nm increases with increasing Cr doping ratio. This behavior can be attributed to the grain growth seen in SEM results, giving rise to less scattering effects from the grain boundaries. Another reason for the increased transmittance that observed for the doped films in the UV/visible light region might be due to change in free carriers. Each incorporated Cr3+ ion brings one free electron in the PbS lattice when substituting the Pb2+ ion thereby increasing the carrier concentration. I.e., Cr atoms substitute Pb atoms and introduce additional free electrons in the parent PbS lattice. Although PbS is a p-type material, however, the Cr-doped PbS nanofilm acts as an n-type semiconducting material due to the incorporation of the Cr donors.
Also, the transmittance spectrum is blue-shifted with an increase in Cr doping concentration.
Based on recorded absorbance (A) and film thickness (d), the absorption coefficient (α) was calculated using the relation:
α = 2.303A/d | (12) |
The type of transition associated with the band structure of PbS can be identified using the following Tauc equation
(αhν)2 = K(hν − Eg) | (13) |
The value of the direct bandgap energy has been calculated from the straight-line portion of the (αhν)2 versus hν curve that intersects the hν axis, as shown in Fig. 5(A). The plot of Eg vs. Cr doping concentration for all samples is displayed in Fig. 5(B). The Eg value of the pure PbS film was found to be equal to 2.196 eV, which matches with the value reported by Barote et al. for PbS thin film deposited by CBD method.49 The PbS-Cr2 film has a bandgap value of 2.422 eV. The Eg value is found to be blue shifted to 2.589 eV for the PbS-Cr6 film, which may be due to the rise in the free carrier concentration. The increase in Eg value with carrier concentration is ascribed to the Moss–Burstein effect, whereas the dopant element increases electrons density in the conduction band thereby lifting the Fermi level.48
Fig. 5 (A) Plots of (αhν)2 versus hν to determine Eg of pure and Cr-doped PbS films, (B) dependence of Eg and D on the level of Cr doping. |
According to the quantum confinement effect, the bandgap widening takes place when the particle size is decreased, as shown in Fig. 5(B). Hence the increasing Eg can be correlated with the decrease in average crystallite size of the main three peaks calculated from XRD data as shown in Table 1. The reduced grain size leads to a reduction of the scattering, and consequently, the optical band increased. In many previous works, the Eg was found to be varying inversely with the crystallite size.50,51 The value of Eg for these sets of films demonstrates that they are good semiconductor candidates for absorbing visible light in optoelectronic and photovoltaic applications.
Fig. 6 Cr-doped PbS electrodes photocurrent density–voltage curves supported on glass under the illumination of 500 W mercury-xenon Lamp without the optical filter. |
From Fig. 6, it can see that the amount of Cr concentration plays a vital role in affecting their PEC properties. The current density is increased from 1.33 to 2.5 mA cm−2 at 1 V as the volume of CrO3 risen from 0 to 6 ml under light illumination. Therefore, PbS-Cr6 is the optimized PEC electrode, which produced the maximum photocurrent and showed the highest PEC properties. Also, it is observed that the photocurrent density increases with applied voltage. The increase in current can be attributed to the small contact height and an increase in tunneling mechanism.52
Although the increasing quantity of Cr impurities in PbS films decreases the light absorption, the efficient charge separation of the electron–hole pairs and suppressed recombination of photogenerated charge carriers of small PbS nanoparticles leading to the rise of photocurrent.53
Also, this increase in Jph can be understood regarding the decrease in the size of the PbS-Cr nanoparticles (Fig. 2) as Cr doping increases. The reduction in the size of the PbS nanoparticles PbS-Cr6 sample will increase the conduction band edge due to a rise in the bandgap of the PbS nanoparticles which would lead to an increase in the driving force for the transfer of photogenerated electrons at the counter electrode.54
The increase of Cr contents induces one free electron into the PbS lattice. So, the carrier concentration increases simultaneously which enhances the photocurrent during water splitting. Also, the conductivity of PbS thin films increases remarkably on doping with Cr.55 Increasing the carrier concentration in the semiconductor reduces the space charge layer width, and to some extent, improves the tunneling probability of electrons across the potential barrier.56 Also, the enhanced charge carrier density can extend the lifetime of charge carriers, giving rise to a reduction in the recombination of the electron–hole pairs.57 In addition, the large surface area of the PbS-Cr6 electrode produces electron–hole pairs of high density, which will motivate the splitting of H2O molecules under the effect of light to carry out the hydrogen generation reaction.
Form the experimental viewpoint; the reproducibility study is significant for approving the obtained data. Fig. 7 illustrated the Jph–E behaviors of the PbS-Cr6 electrode was measured in the dark and under the illumination of 500 W mercury-xenon lamp without an optical filter for many repeats. From this figure, the Jph values for the PbS-Cr6 electrode are measured six times with relative standard deviation (RSD) of 0.63% and a mean value of 2.48 mA cm−2. Also, the photoelectrode shows a quite low dark current and negligible concerning their respective photocurrent, indicating no fierce electrocatalytic water splitting occurs.53
Fig. 7 Reproducible studies of photocurrent density–voltage curves of the PbS-Cr6 electrode in dark and under white light illumination without the optical filter. |
The photostability of the PbS-Cr6 electrode is investigated for an elongated time and shown in Fig. 8. During these measurements, a small bias voltage of 0.85 V is introduced between the electrodes to overcome any external losses of the measuring system. From Fig. 8, the Jph values are decreased in the first period due to the minimal corrosion that occurs as a result of the first reaction of the electrode with the electrolyte. Also, the high surface density of states maybe results in a significant pinning of the Fermi level that can facilitate the participation of these defect states in the surface oxidation process, leading to small degradation of the PbS-Cr6 electrode. Above 200 s, the Jph values remain constant nearly at 0.42 mA cm−2 due to increasing the accumulation of the ionic charges. Doping PbS film with Cr impurities leads to an increase of surface area and a decrease in the electron/hole recombination rate. Therefore, the significant increase in the photostability of PbS-Cr6 photoelectrode allows the reusability of the PbS-Cr6 for several runs. This result is suggesting that the photoanode has high chemical stability and a long lifetime to work in the H2 production cell.
The variation of Jph with the applied potential under the illumination of monochromatic light for the electrode is shown in Fig. 9. The average intensity of the incident monochromatic light was 50 mW cm−2. The Jph values decrease with increasing the optical wavelength from 390 to 636 nm. The photoelectrochemical Jph for water splitting has maximum and minimum values of 1.63 and 1.41, respectively. As the optical wavelength of the incident light decreased, the required potential for the photoelectrochemical generation decreases due to the photon energy increase.
Fig. 9 Photocurrent-voltage curves of the PbS-Cr6 electrode under the illumination of monochromatic light. |
The PEC performance of the PbS-Cr6 electrode is evaluated by measuring the incident photon-to-current conversion efficiency (IPCE) and photon-to-current efficiency (ABPE) under monochromatic illumination conditions. The IPCE analytical measurements give meaningful insight into the contribution of the PbS-Cr6 film in the conversion efficiency of the incident photons into charge carriers. A higher value of IPCE signifies improved transportation of photoexcited charge carriers. The IPCE is determined at an applied potential of 1 V from eqn (14).58
(14) |
Based on the optical behavior of the PbS-Cr6 film, the prepared electrode has an optimum IPCE% value of 13.5% at 390 nm, then this value decreases with increasing the wavelength to reach 7% at 636 nm as shown in Fig. 9(A).
The ABPE represents the development of the photoelectrode performance as a function of the applied potential. It measures the photoconversion efficiency of light energy to chemical energy. The ABPE efficiency values for the designed photoelectrodes are calculated by using eqn (15):59
(15) |
Photoelectrode | Performance |
---|---|
Cr-doped PbS | Jph = 1.5 mA cm−2, IPCE = 13.5%, ABPE = 1.44% at 390 nm (present study) |
Trimethylphenylporphyrin | Jph = 0.1 mA cm−2, IPCE = 0.028% (ref. 60) |
ITO/PMPDI/CoOx | Jph = 0.15 mA cm−2, IPCE = 1% at 1.6 V (ref. 61) |
CuNb3O8 | IPCE = 6–7% at λ > 420 nm (ref. 62) |
Ag-doped CaFe2O4 | IPCE = 3.8% (ref. 63) |
Si-doped InGaN-based nanowire | Jph = 1.42 mA cm−2, ABPE = 0.9% at 1.5 V (ref. 64) |
Au/TiO2 nanotube | IPCE = 8% (ref. 65) |
TiO2 nanotube | Jph = 1.5 mA cm−2, ABPE = 0.84% at 100 mW cm−2 (ref. 66) |
InGaN/GaN nanowire | Jph = 1.8 mA cm−2, IPCE = 9% at 1 V (ref. 67) |
The effect of temperature from 30 to 70 °C on the PbS-Cr6 electrode for H2 generation is shown in Fig. 10(A). From this figure, the Jph values increase with increasing temperature due to the increased mobility of ions. So the increase in temperature increases the H2 generation process. So the rate of H2 generation under different temperatures is related to the Jph values. The relation between reciprocal of temperature and Jph values (rate of reaction) is represented in Fig. 10(B). From this relation, the Ea can be calculated using the Arrhenius equation. From the slope value, the Ea value is 24.32 kJ mol−1. This value is small, so the prepared electrode is very efficient for the H2 generation reaction. In addition, the enthalpy ΔH* and entropy ΔS* for the H2 generation reaction can be calculated using the Eyring equation and Fig. 11. From the slope and intercept values, the ΔH* and ΔS* values are 66.22 J mol−1 and −199.51 J K−1 mol−1, respectively.
Fig. 11 (A) The effect of temperature on H2 generation process, (B) plot of the Jph against reciprocal of temperature, and (C) plot of Jph/T versus reciprocal of reciprocal temperature. |
This journal is © The Royal Society of Chemistry 2020 |