aCain Department of Chemical Engineering, Louisiana State University, Baton Rouge, LA 70803, USA. E-mail: carges@lsu.edu
bApplied Materials Division, Argonne National Laboratory, Lemont, IL 60439, USA. E-mail: yplin@anl.gov
First published on 4th March 2020
Electrochemical separation processes are undergoing a renaissance as the range of applications continues to expand because they offer opportunities for increased energy efficiency and sustainability in comparison to conventional separation technologies. Existing platforms such as electrodialysis and electrodeionization (EDI) are seeing significant improvement and are currently being deployed for treating a diverse set of liquid streams (e.g., water and wastewater treatment, organic acid separation, etc.). In addition, the relatively low inherent electricity requirement for electrochemical separations could potentially be satisfied through integration with sustainable sources of renewable energy. In order to achieve a truly sustainable electrochemical separations process, it is paramount to improve the energy efficiency of electrochemical separations by minimizing all sources of resistances within these units. This work reports of a new class of symmetric and asymmetric Janus bipolar resin wafers (RWs) that augment the spacer channel ionic conductivity in EDI while having the additional functionality of splitting water into protons and hydroxide ions. The latter attribute is important in niche applications that require pH modulation such as silica and organic acid removal from liquid streams. The Janus bipolar RWs were devised from single ion-conducting RWs that were interfaced together to create an intimate polycation–polyanion junction. Interestingly, the conductivity of the single ion-conducting RWs at low salt concentrations was observed to be dependent on the ionic mobilities of the counterions that the RW was transferring. Using single ion-conducting RWs to construct Janus bipolar RWs enabled the incorporation of a water-splitting catalyst (aluminum hydroxide nanoparticles) into the porous ion-exchange resin bed. To the best of our knowledge, this is the first time a water dissociation catalyst has been implemented in the ion-exchange resin bed for EDI. The water dissociation catalyst in bipolar junctions pre-polarizes water making it easier to split into hydronium and hydroxide ion charge carriers under applied electric fields via the second Wien effect. The new molecularly layered Janus RWs demonstrate both satisfactory water-splitting and salt removal in bench scale EDI setups and these materials may improve, or even supplant, existing bipolar membrane electrodialysis units that currently necessitate large electrolyte feed concentrations.
Design, System, ApplicationBipolar membranes are the standard-bearer material for pH adjusting process streams without the addition of acids and bases in electrodialysis. These membranes feature weak-acid or -base catalysts that pre-polarize water at the polycation–polyanion interfaces making it susceptible for splitting into hydronium and hydroxide ion charge carriers under electric fields. Further, they require intimate polycation–polyanion interfaces as large distances between the fixed charges compromise water-splitting efficiency. A limitation of bipolar membrane electrodialysis (BPMED) is the need for concentrated salt feeds to overcome significant ohmic resistances in the diluate chamber. This work engineered a new class of porous, Janus ion-exchange resin wafers (RWs) featuring bipolar junctions with aluminum hydroxide (Al(OH)3) nanoparticles as the water dissociation catalyst. These RWs have a flexible material design as the Al(OH)3 catalyst can be incorporated into different layers and can have tuned polycation–polyanion molecular interfaces through application of thin film ionomer coatings. The Janus bipolar RWs augmented the diluate chamber ionic conductivity in electrodeionization (EDI) setups, overcoming limitations experienced in BPMED, while also co-currently splitting water and removing chloride ions. It is envisioned that the Janus bipolar RWs will be useful in niche water treatment applications that require pH adjustment – e.g., silica and organic acid removal. |
An important sub-subset of separations relates to electrochemical systems that are effective for removing ionic species from aqueous and non-aqueous liquids. Such processes are used in industrial wastewater remediation and deionization. Electrochemical systems for ionic species removal from liquid streams include well-established platforms such as electrodialysis (ED)3 and electrodeionization (EDI)4–7 and emerging ones such as membrane capacitive deionization/capacitive deionization (MCDI/CDI)8–11 and shock electrodialysis.12,13 Electrochemical separations have also been used for purifying gases through electro-swing reactive14 and RW-EDI gas adsorption.15
A key component for realizing high energy efficiency and high performance in electrochemical separations is minimizing sources of resistance through adjustment of the system's operating parameters and implementation of new materials. For example, Lin et al. were able to optimize the system parameters (e.g., cell voltage and feed concentration flow rate) for RW-EDI to make it more energy efficient than reverse-osmosis (RO) for brackish water treatment (2000 ppm of total dissolved solids (TDS) to 5000 ppm of TDS in the feed concentration).16 As a materials example, Palakkal et al. showed that reducing the ion-exchange membrane (IEM) materials' area-specific resistance (ASR) by a factor of 5 to 10 resulted in a 50% reduction in energy consumption for desalination at low TDS concentrations (e.g., 250 ppm to 540 ppm).17 Hence, both materials innovation and systems level engineering enhanced energy efficiency for electrochemical separations.
A uniquely defining phenomenon in the EDI process is the regeneration of the ion-exchange resin beads during deionization through water-splitting. Unlike ion-exchange chromatography, EDI can be implemented as a continuous ion-exchange process because water-splitting, which results in the formation of hydroxide (OH−) ions and protons (H+), occurs in the ion-exchange resin bed. These ions can exchange back into the anion exchange and cation exchange resin (AER and CER) particles, respectively, recombine to form water, or migrate out of the diluate chamber via the anion exchange and cation exchange membranes (AEMs and CEMs). Hence, the water-splitting phenomenon allows for continuous ion-exchange and removal of charged species from the liquid feed stream. Ion-exchange chromatography, on the other hand, requires acid and base chemicals for regenerating the ion-exchange resin particles in the column. The use of these chemicals leads to undesirable waste, downtime for the regeneration/cleaning process, and higher capital costs because multiple columns need to be installed in parallel to ensure a continuous process.
Water-splitting in EDI has been well-documented;4,18 however, it has been primarily discerned by monitoring the pH changes of the effluent streams. In a continuous EDI process (see Fig. 1A), the ions in the aqueous solution are adsorbed via ion-exchange onto the resin beads. These adsorbed ions are then successively desorbed from the adsorption sites by two parallel phenomena: i.) electrically-driven migration and ii.) resin bead regeneration caused by H+ and OH− ions that are generated from water-splitting. More specifically, the desorbed salt ions exchanged by the OH− and H+ ions electro-migrate into the concentrate compartment, which is separated by the ion-exchange membranes. At steady-state, there is constant concentration profile along the direction of feed flow for ions adsorbed on the ion-exchange resin beads to the ion-exchange membrane surfaces. In a continuous EDI process, the bulk of deionization occurs at the entrance to the middle region of the unit. As the concentration of mobile ions in the diluate stream decreases, the ion-exchange bed augments the diluate stream conductivity. Finally, water-splitting at the middle to the end of the chamber regenerates the ion-exchange resin particles and provides ions to enable electrical current flow through the EDI unit despite the majority of salt ions already being removed.4,19
The water-splitting phenomenon in EDI occurs at the interface of CER and AER particles that are in intimate contact and form a p–n type abrupt junction.20 This junction of interfaced polycations and polyanions is designated as the bipolar junction (highlighted in Fig. 1B). Applying an external electric field gradient across the bipolar junction interface leads to water-splitting.21 It is important to note that the depletion width for bipolar junction interfaces is few nanometers.22 Therefore, large distances between the oppositely charged particles hinder water-splitting in the ion-exchange resin beds of EDI. Further, a small population of bipolar junctions in the ion-exchange resin particle bed minimizes the water-splitting effect leading to poor regeneration of ion-exchange resin particles. Conversely, increasing the number of bipolar junctions within the RW accelerates proton and hydroxide formation. Regardless of the electrochemical separation process, the water-splitting generated in the resin bed can be exploited to achieve a desired pH adjustment of the process stream (e.g., during deionization, electrocoagulation of metals23 and silica,24 gas capture,15 and mineral acid and base production25,26). For example, the maintenance of an alkaline solution can ensure that organic acids remain in ionized form for separation based upon anion exchange; this is important for carbon valorization and purifying bio-fuels.27 BPM electrodialysis25,26 has been the most common method for electrochemical pH adjustment of process streams, but this method necessitates fairly concentrated streams of TDS to overcome spacer channel ohmic resistances to electrochemically transport the ions.
This paper, for the first time, demonstrates the incorporation of a water dissociation catalyst into ion-exchange RWs for promoting water-splitting in RW-EDI. Water dissociation catalysts, which are found in bipolar membranes, facilitate water-splitting via the second Wien effect28 (depicted in Fig. 1B). The catalyst in the bipolar junction pre-polarizes water to severe its HO–H bond. Mallouk and co-workers29 recently reported that the catalyst can dampen the strength of the electric field in the bipolar junction region for splitting water, but this undesired attribute is overshadowed by the importance of the catalyst that promotes water-splitting kinetics by several orders of magnitude – when compared to a bipolar junction with no catalyst. A previous effort30 by our group attempted to incorporate a water dissociation catalyst31,32 into immobilized ion-exchange RW used in EDI was unsuccessful as incorporation of the aluminum hydroxide (Al(OH)3) nanoparticles, a water dissociation catalyst, compromised the mechanical integrity of the RW. To overcome this challenge, a layered manufacturing approach was adopted by 1) preparing a single ion-conducting RW, 2) depositing of Al(OH)3, and 3) adjoining oppositely charged, single ion-conducting RW or a thin layer of oppositely charged ionomer film. These designs are termed symmetric Janus bipolar RW and asymmetric film Janus bipolar RW, respectively.
Prior to investigating the water-splitting behavior of the Janus bipolar RWs, the ionic conductivity of the single ion-conducting RWs were studied. Both single ion-conducting RWs featured an ionomer binder, and these wafers showed superior ionic conductivity over the RW that consisted of mixed AER and CER and a PE binder (i.e., the benchmark material used at Argonne National Laboratory). The anion exchange ionomer (AEI) binder with AER RW (AEI–AER RW) displayed the highest ionic conductivity to date of all RW materials reported in the literature16,30,33 (17 ± 0.3 mS cm−1 at 0.1 g L−1 in NaCl to 58 ± 3.6 mS cm−1 at 29 g L−1). Interestingly, the CEI binder with CER RW (CEI–CER RW) exhibited lower ionic conductivity in comparison to the AEI–AER RW. Furthermore, addition of CER to AEI binder RW (AEI–CER RW) also resulted in lower ionic conductivity in comparison to the AEI–AER RW. These observations are primarily attributed to the lower ionic mobility of the Na+ counterion in the CER when compared to the Cl− counterion in the AER. Hence, the ionic conductivity is largely influenced by both the ion-exchange resins and the ionomer binder.
With the newly prepared single ion-conducting RWs, the water-splitting behavior of the RWs with and without a water dissociation catalyst and different configurations (e.g., symmetric and asymmetric) were studied. The incorporation of a water dissociation catalyst improved water splitting by factor of 2–4 while providing a similar level of ionic conductivity and porosity in comparison to the RWs without the catalyst. The Janus bipolar RW with a water dissociation catalyst caused significant pH shifts in the diluate and concentrate compartments of EDI that are similar to what is observed in bipolar membrane electrodialysis.25,26 The Janus bipolar RW is an alternative material for pH adjustment of the concentrate and diluate streams in EDI rather than using a BPM. Notably, it can have tailored molecular interfaces located at different junctions across the wafer thickness for modulating pH adjustment of streams to different values.
(1) |
(2) |
(3) |
(4) |
(5) |
Fig. 2 (A) Illustration of single ion-conducting RWs. (B) Manufacturing scheme for single anion- and single cation-conducting RWs. |
Fig. 2B illustrates the manufacturing process of the single ion-conducting RWs. AEI and CEI binders were prepared as described elsewhere.30 The 1H NMR of the AEI and CEI binders and IEC values of the RWs are presented in Fig. S1a–c† and Table 1. AERs and CERs were vacuum dried at room temperature for 30 minutes prior to use to remove moisture. The ionomer was dissolved to form a 14 wt% concentration in N-methyl-2-pyrrolidone (NMP) solvent. The ionomer solution was mixed with the ion-exchange resins and sodium chloride (a sacrificial porosigen) in a 2:2.4:1 ratio and then cast into a foil-lined stainless-steel mold. The mold was dried in an oven at 60 °C for 12 hours to remove residual solvent and then hot pressed at 2 metric ton load for 125 °C for 1.5 hours for the CEI–CER or 150 °C for 2 hours for the AEI–AER. The RWs were cooled under the 2-metric ton load before removing from the molds and then immersed in DI water three times for 20 minutes to dissolve the porosigen (i.e., NaCl).
Resin wafer type | IEC (meq g−1) | IEC (meq mL−1) | Porosity (%) |
---|---|---|---|
CEI–CER | 1.07 | 1.00 | 13.5 ± 1.6 |
AEI–AER | 1.25 | 0.99 | 16.6 ± 1.5 |
AEI-mixed | 1.36 | 0.96 | 18.6 ± 3.4 |
AEI–CER | 1.50 | 0.99 | 13.0 ± 1.9 |
PE-mixed | 0.73 | 0.82 | 15.7 ± 1.2 |
Symmetric Janus with catalyst | 0.99 | 1.05 | 16.7 ± 3.5 |
Symmetric Janus without catalyst | 1.14 | 0.91 | 15.6 ± 3.2 |
In our previous work,30 SPEEK based CEI binder produced mechanically stable RWs with a CER–AER mixture and AER only. However, the CEI binder with the CER only resulted in a mechanically fragile RW (see Fig. S2†) indicating that binder and ion-exchange resin compatibility are important properties for making robust RWs. Our previous work showed that quality RWs could not be produced from perfluorosulfonic acid binders (e.g., Nafion®), and sulfonated polystyrene binders, suggesting that it was necessary to modify the manufacturing procedure for the CER RW by blending PE binder with the SPEEK ionomer solution (1:1 mass ratio). This manufacturing procedure produced a robust, free-standing cation-exchange RW shown in Fig. 2B.
The AEI–AER RW (indicated by the black squares in Fig. 3A) displayed higher ionic conductivity in comparison to CEI–CER RW (indicated by the blue diamonds in Fig. 3A) and mixed RW (indicated by the green triangles in Fig. 3A) featuring either AER or CER due to a higher ionic mobility for Cl− over Na+ in dilute water streams36 (7.91 × 10−4 cm2 s−1 V−1 for Cl− and 5.194 × 10−4 cm2 s−1 V−1 for Na+ − i.e., about 50% higher for chloride). Ionic mobility represents the migration rate of an ion in the presence of an applied electric field, and it is proportional to the diffusion coefficient normalized to the thermal energy of the system.
Fig. 3B presents the ionic conductivity of the RW samples normalized to their IEC values. Ionic conductivity is linearly dependent on the concentration of fixed charger carriers in the ion-exchange material.37 Thus, a material with a higher IEC would result in higher ionic conductivity. The AEI–AER still displayed the highest ionic conductivity when normalized to IEC at low NaCl concentrations. The ionic conductivity for single ion-conducting RWs is attributed to two factors: i) counterion migration along the polymer in the ion-exchange resin and ionomer binder and ii) ionic migration of the supporting electrolyte (i.e., NaCl) dissolved in the RW sample. By normalizing the ionic conductivity to the IEC, it is clear that the AEI–AER displays greater ionic conductivity because the counterion, Cl−, has a higher ionic mobility than Na+.
In the context of most electrochemical separation platforms, deionization occurs by transport of anions and cations across an AEM or CEM, respectively. The rate of ion removal is dependent upon the rate of delivery of ions to these interfaces, and thus, the ionic mobility values in the aqueous phase and ion-exchange resin bed are important descriptors for EDI transport. Because of iso-neutrality constraints, the ratio of cations to anions (assuming both have the same valence number) must be equivalent in the diluate and concentrate chambers. Hence, the rate of both anion and cation removal from the diluate chamber is limited by the slowest moving ion. Based on the ionic conductivity results from single ion-conducting RWs, it seems that improving deionization of NaCl from water with RW-EDI requires a strategy to promote Na+ conductivity. Since ionic mobility is an intrinsic property of the ion itself, an alternative strategy for further research would be to increase the IEC of the CER in order to improve Na+ conductivity and the overall efficiency of EDI. Other strategies, such as molecular engineering of the RW materials (e.g., percolating pathways of ionic channels),38 may also be another effective means for promoting Na+ conductivity.
Fig. 4 Cross-sectional views of (A) symmetric and (B) asymmetric Janus bipolar resin wafers used in this report and concepts of a (C) reversed asymmetric and (D) bilayer Janus bipolar resin wafer. |
Fig. 5A illustrates the layering method used to manufacture a symmetric Janus bipolar RW. In this approach, the initial CEI–CER layer was prepared as described in Fig. 2B; however, the final submersion in DI water was omitted. After preparing the CEI–CER RW, a uniform layer of aluminum hydroxide (Al(OH)3) nanoparticles (10 wt% of particles suspended in DI water) was applied on to the CEI–CER layer with a final loading of 0.034 g cm−2. The catalyst layer was deposited in three applications and allowed to dry for 30 minutes after each application. The CEI–CER layer was inserted into a foil-lined stainless-steel mold, and the AEI–AER mixture described in Fig. 2B was layered on top. The symmetric Janus bipolar RW was dried at 60 °C for 12 hours, hot pressed at 150 °C for 1.5 hours, and allowed to cool under load to room temperature. The final symmetric Janus bipolar was submerged in DI water for a total of 1 hour, during which the water was exchanged three times to remove the porosigen. A photo of the symmetric Janus bipolar RW is shown in Fig. 5A. The darker and lighter sides of the RW correspond to the cation and anion exchange layers, respectively.
The second manufacturing method for preparing the asymmetric Janus bipolar RW is shown in Fig. 5B. Unlike the symmetric RW, the AEI–AER was first prepared as detailed in Fig. 2B, omitting the water immersion step. Next, the water dissociation catalyst was added in the same fashion as described for Fig. 5A. Rather than applying the oppositely charged CEI–CER on top of the AEI–AER with a water dissociation catalyst, a thin film of SPEEK ionomer was deposited through three applications of spray deposition (10 wt% SPEEK in NMP) with a final loading of 0.14 g cm−2. The rationale for selecting the asymmetric Janus bipolar RW variant was based on i) the previous ionic conductivity results, which showed that the AEI–AER had the highest ionic conductivity (Fig. 3A), and ii) the straightforward nature of this manufacturing procedure, which involved fewer processing steps to incorporate a bipolar junction and water dissociation catalyst.
Fig. 6A–D. present the electron micrographs, with and without EDX mapping, at the interface between cation exchange and anion exchange groups in the symmetric Janus bipolar RW that did not contain a water dissociation catalyst. Fig. 6A confirms successful integration of the AEI–AER and CEI–CER; the two porous layers are in contact with each other. Elemental mapping for sodium and chlorine in these micrographs, Fig. 6B and C respectively, revealed separate and distinct cation and anion exchange layers (i.e., an abrupt, oppositely charged molecular bipolar junction interface). Sodium is the counterion to the tethered sulfonate groups in the CEI–CER material, while chloride is the counterion for the tethered quaternary ammonium groups used in the AEI–AER. Fig. 6D shows the EDX mapping for sulfur, which is present as sulfonic groups CER and CEI, and as a minor component in AEI due to the poly(arylene ether sulfone) backbone. As a result, a stronger signal for sulfur is evident in the CEI–CER layer in comparison to the AEI–AER layer.
When manufacturing the symmetric Janus bipolar RW, it was discovered that the mechanical-thermal lamination press time was a critical parameter. EDX mapping indicated that excessive press times, such as 2 hours or greater, resulted in mixing of CEI and AEI binders and precluded the formation of an abrupt bipolar junction layer. A 1.5 hour press time at 150 °C was determined to be ideal because it yielded an intimate, but distinct, bipolar junction. Although quantifying the effects of press time on the interface were outside the scope of this work, measuring the electrochemical properties of the bipolar junctions could provide a better understanding of the structure, property, and performance relationships for these materials. In this study, the focus was limited to adjoining the two different RWs into one mechanically robust RW (i.e., the symmetric Janus bipolar RW sample). With a successful manufacturing scheme in place, the Janus bipolar RW with a water dissociation catalyst was prepared and imaged with SEM and EDX mapping (Fig. 6E and F). From these SEM images, it is evident that the sodium and chlorine layers are separated by an aluminum layer at the interface.
The addition of the Al(OH)3 water dissociation catalyst into the symmetric and asymmetric Janus bipolar RW samples increased their ionic conductivity values to those comparable with the AEI–AER RW at low NaCl concentrations (<3 g L−1). At higher NaCl concentrations (>3 g L−1), the Janus bipolar RWs had slightly higher ionic conductivity values when compared to the AEI–AER. The increase in ionic conductivity with the addition of Al(OH)3 into the RW was unexpected because the Al(OH)3 does not contain any formal ionic charges. However, Al(OH)3 can accept an OH− from solution to form an ionic pair between Al(OH)4− and H+. If these ionic pairs exist in small populations on the nanoparticle surfaces, they could potentially augment the ionic conductivity of the RW sample. To further explore this hypothesis, Al(OH)3 nanoparticle suspensions were prepared with various concentrations, and the solutions' ionic conductivities were measured using a conductivity probe (Fig. S4†). At 0.2 M, Al(OH)3 nanoparticle suspension exhibited a moderate ionic conductivity value of 0.53 mS cm−1 suggesting the formation of Al(OH)4− on the nanoparticle surface. It is difficult to quantify the exact concentration of the nanoparticles in the RW samples, but it is lower than 0.2 M (which was measured as suspension in DI water), and the addition of the Al(OH)3 nanoparticles into the Janus bipolar RW samples resulted in a nearly two-fold increase in ionic conductivity (i.e., 7 to 10 mS cm−1) in comparison to the non-catalyst containing samples. It is also unlikely that the increase in ionic conductivity was attributed to water-splitting because the cell voltage during electrochemical impedance spectroscopy was small (<1 mV). While the formation of a surface charge on the Al(OH)3 nanoparticles is plausible, further investigations are warranted to better understand the increase in RW ionic conductivity with a water dissociation catalyst.
Owing to the small changes on a logarithmic scale, pH values were converted to H+ in the concentrate and OH− in the diluate (Fig. 9B and C). From these plots, it is clear that the increase in acidity in the concentrate and alkalinity in the diluate is greater by a factor of 3–4 for a Janus bipolar RW sample containing a water dissociation catalyst. The reduction in diluate alkalinity over time resulted from the depletion of Cl− (near 80% removal) from the diluate chamber (Fig. 9D) and thus, continual deionization required removal of accumulated OH− in the diluate chamber through the AEM to maintain electrical current flow in the EDI.
Aside from changes in pH, desalination performance was evaluated for asymmetric Janus bipolar RWs both with and without water splitting catalyst. Fig. 9D shows that as expected in both cases, the Cl− concentration in the diluate compartment decreased with time while the Cl− concentration in the concentrate compartment increased with time. The Cl− concentration profiles for wafers with and without the water splitting catalyst were not significantly different, which suggest that the inclusion of the catalyst does not necessarily facilitate Na+ or Cl− ion transport. This can be attributed to the 3–7 higher ion mobility for H+ and OH− in comparison to Na+ and Cl− in water,36 which have been reported to parallel the trends in ion-exchange resins.41
In summary, the EDI tests showed that asymmetric Janus bipolar RWs featuring Al(OH)3 as a water dissociation catalyst promoted greater water-splitting in comparison to similar Janus bipolar RWs that lack the catalyst but did not affect Cl− deionization. Overall, these results imply that Janus RW materials may be an appropriate substitute for EDI processes that utilize BPMs, analogous to BPM electrodialysis but without the requirement of having to use high feed concentrations to minimize spacer channel resistances.
Additionally, Janus bipolar RWs were explored by the development of the single ion-conducting of RWs. The addition of a water dissociation catalyst into a molecularly intimate polycation–polyanion bipolar junction interfaces located in porous RW materials was investigated for the first time. The water dissociation catalyst enhanced the conductivity of the RW, and these Janus wafers rivaled the conductivity of the most conductive single ion-conducting RW (AEI–AER). The EDI demonstration of the asymmetric Janus RW showed that these materials can be utilized to modify the solution pH and suggest that pH control with RW material could be useful to enable future electrodeionization separation technologies that may compete with bipolar membrane electrodialysis.
Footnotes |
† Electronic supplementary information (ESI) available: 1H NMR data of ionomer binders and precursors. Supplemental ionic conductivity data of the RWs and Al(OH)3 nanoparticle suspension. Material specifications and conventional (benchmark PE-mixed) RW preparation. See DOI: 10.1039/c9me00179d |
‡ Contributed equally to this report. |