aHenan Joint International Research Laboratory of New Energy Storage Technology, Key Laboratory of Microelectronics and Energy of Henan Province, School of Physics and Electronic Engineering, Xinyang Normal University, Xinyang 464000, P. R. China. E-mail: luyang.181@163.com; ysluo@xynu.edu.cn; Fax: +86 376 6390801; Tel: +86 376 6390801
bCollege of Chemistry and Chemical Engineering, Luoyang Normal University, Luoyang 471934, P. R. China
cCollege of Physics and Electronic Engineering, Nanyang Normal University, Nanyang 473061, P. R. China
First published on 5th March 2022
The industrialization and commercialization of Li–S batteries are greatly hindered by several defects such as the sluggish reaction kinetics, polysulfide shuttling and large volume expansion. Herein, we propose a heteroatom doping method to optimize the electronic structure for enhancing the adsorption and catalytic activity of VN that is in situ embedded into a spongy N-doped conductive framework, thus obtaining a Co-VN/NC multifunctional catalyst as an ideal sulfur host. The synthesized composite has both the unique structural advantages and the synergistic effect of cobalt, VN, and nitrogen-doped carbon (NC), which not only improve the polysulfide anchoring of the sulfur cathode but also boost the kinetics of polysulfide conversion. The density functional theory (DFT) calculations revealed that Co doping could enrich the d orbit electrons of VN for elevating the d band center, which improves its interaction with lithium polysulfides (LiPSs) and accelerates the interfacial electron transfer, simultaneously. As a result, the batteries present a high initial discharge capacity of 1521 mA h g−1 at 0.1 C, good rate performance, and excellent cycling performances (∼876 mA h g−1 at 0.5 C after 300 cycles and ∼490 mA h g−1 at 2 C after 1000 cycles, respectively), even with a high areal sulfur loading of 4.83 mg cm−2 (∼4.70 mA h cm−2 at 0.2 C after 100 cycles). This well-designed work provides a good strategy to develop effective polysulfide catalysis and further obtain high-performance host materials for Li–S batteries.
New conceptsSmooth trapping, diffusion and conversion of lithium polysulfides by various catalysts is a promising strategy for restraining the shuttle effect in Li–S batteries. However, most conventional catalysts have their own inevitable drawbacks that reduce the capture or conversion efficiency of LiPSs. Heteroatom doping is an effective modification method to complement the shortcomings of catalysts. In this work, we design a cobalt-doped vanadium nitride nanocrystal embedded in a conductive carbon framework, aiming to simultaneously enhance the adsorption and catalytic performance of VN catalysts for polysulfides. Density functional theory calculations and experimental results jointly demonstrated the enriched d orbit electrons and embellished bandgap of VN by cobalt doping, further improving the reaction kinetic behaviors of LiPSs. This heteroatom doping strategy provides a unique insight for constructing catalysts with optimized adsorption and interfacial charge transfer capability in Li–S batteries. |
Among these candidates, vanadium nitride (VN) stands out as one of the most promising sulfur host materials because of its robust electrochemical corrosion resistance and remarkable electronic conductivity (1.17 × 106 S m−1 at room temperature)12 More significantly, VN possesses similar catalytic properties to noble metals that may facilitate the conversion from long-chain polysulfides (Li2Sn, n ≥ 4) to short-chain Li2S2/Li2S and further improve the reaction kinetics.12 Nevertheless, owing to the anion species occupying the interstitial sites of lattices, the trapping ability toward LiPSs of metal nitrides is much weaker than that of metal oxides, leading to a compromise of trapping and conversion efficiency.13,14 To enhance the adsorption ability of VN with LiPSs, Co atom doping is a promising material modification strategy, which could engineer the electronic structure by increasing d electrons.15–17 However, Co-doped VN has a strong tendency of aggregation through hydrothermal reaction, and this large-size electrocatalyst with a limited area of the reactive interface leads to the partial loss of sulfur active material.18,19 In consequence, the synthesis of ideal catalysts with smaller particle sizes, richer reaction interfaces, appropriate adsorption ability and ultra-high catalytic activity remains a critical challenge.
With careful consideration of the metal heteroatom doping effect and catalyst interface design, a N-doped graphitic carbon framework embedded with Co-VN nanocrystals (Co-VN/NC) is synthesized as an efficient polysulfide adsorber and convertor through a facile template-assisted strategy. Here, the NaCl crystal as a template can be removed by deionized water, the glucose acted as a C source to structure the 3D porous carbon framework, and the NH4VO3, urea and Co(NO3)2·6H2O were the V, N and Co source, respectively. Notably, the introduction of Co element could enrich the d orbit electrons of VN, and further redistribute the d-band center and embellish the bandgap, which can improve the affinity toward LiPSs. Moreover, the widespread ultrasmall Co-VN particles offer abundant triple-phase interfaces (between catalyst, conductive substrate and electrolyte) for rapid surface reactions of LiPSs and accelerating Li2S uniform nucleation and growth. Furthermore, the N doping of the graphitic carbon conductive network provides more electric contact sites for rapid surface electronic exchange, and improves the surface wettability for reducing the polarization resistance of the sulfur cathode. As a result, the 3D Co-VN/NC cathodes yield a remarkable cycling performance with a decay rate of 0.043% per cycle over 1000 cycles at 2.0 C, and delivered a high areal capacity of 4.98 mA h cm−2 even with a sulfur loading of 4.83 mg cm−2.
Ead = Etotal − Esuf − ELi2Sn | (1) |
(2) |
Fig. 1 Schematic illustration of the template-assisted strategy for the synthetic route of the 3D Co-VN/NC framework. |
The surface morphologies of the NC, VN/NC and Co-VN/NC are displayed in Fig. 2. As shown in Fig. 2a1–a2, the NC sample displays a 3D porous structure consisting of an interconnected ultrathin carbon backbone. After the addition of NH4VO3 and Co(NO3)2·6H2O, the structures of VN/NC and Co-VN/NC still keep the honeycomb-like porous framework (Fig. 2b1 and c1), and the VN and Co-VN nanocrystals are uniformly distributed on the walls of graphitic carbon as shown in the higher magnification images (Fig. 2b2 and c2). Moreover, thermogravimetric analysis in Air suggests that the content of Co-VN in Co-VN/NC is about 39.9% (Fig. S2a, ESI†).23,24 To verify the functions of melamine and urea, we also synthesized samples through similar comparative experiments. When the sample is normally annealed without adding melamine, the final product is a carbon composite material with no obvious VN crystal particles on the surface, and the XRD test result also showed no diffraction peak of vanadium nitride (Fig. S2b and c, ESI†). The corresponding XPS data of the control sample without adding melamine are also given. The XPS spectrum (Fig. S2e and f, ESI†) demonstrates the presence of nitrogen-doped carbon in the obtained sample, but this may be due to the nitrogen source provided by urea and NH4VO3 (). The above results prove that melamine is the main nitrogen source of VN. Without urea, the synthesized sample still contains VN, but the concentration of the precursor solution changed, which led to the fracture of the three-dimensional carbon network structure (Fig. S2b and d, ESI†). In addition, considering that NH4VO3 can be pyrolyzed to produce NH3, 3D NC was prepared without adding melamine, NH4VO3 and Co(NO3)2·6H2O in the normal annealing process. And the high-resolution XPS spectra of N 1s and C 1s were obtained for the 3D NC sample, which proved that nitrogen was successfully doped into the carbon material (Fig. S2g and h, ESI†). In summary, we believe that urea is a nitrogen source of nitrogen-doped carbon and also supports the 3D structure of the carbon network.
The structural morphology of Co-VN/NC was further elucidated by TEM. As shown in Fig. 2d, the 3D network structure formed via the ultrathin carbon walls was robustly interspersed with Co-VN nanoparticles, which was consistent with the SEM images. And the statistical data inset of Fig. 2d indicated that the size of the Co-VN nanocrystals ranged from 9 to 20 nanometers. A representative HRTEM image is shown in Fig. 2e, disclosing lattice fringes with a spacing of 0.24 and 0.21 nm, which corresponded to the (111) and (200) planes of VN, respectively.25,26 In addition, the elemental mapping images (Fig. 2f) reveal the homogeneous distribution of vanadium, nitrogen, cobalt and carbon elements in the 3D Co-VN/NC framework. As shown in Fig. S3 (ESI†), the energy dispersive X-ray (EDX) analysis reveals that the molar ratio of N to V elements is about 1.23:1, and the excess nitrogen element comes from the nitrogen-doped carbon network.
The crystal structures of the Co-VN/NC, VN/NC and NC were identified by X-ray diffraction (Fig. 3a). Four Bragg reflection peaks at 37.6°, 43.7°, 63.6°, and 76.3° are assigned to the (111), (200), (220), and (311) lattice planes, respectively.27 All diffraction peaks were well indexed to cubic VN (Fm3m, JCPDS No. 73-0528), with the wide peak around 26° corresponding to amorphous carbon.28 Meanwhile, the XRD patterns (Fig. 3b) of Co-VN/NC display peaks at 76.4°, significantly positively shifted to a higher angle compared to that of VN/NC, which is due to the atomic radius of cobalt being smaller than that of vanadium.29,30 In addition, the intensity of the XRD peaks reduces and also becomes broader, illustrating the successful doping of Co into the VN crystal lattice.31
X-ray photoelectron spectroscopy (XPS) was used to investigate the surface composition information of Co-VN/NC and the nature of the dopants. The full XPS spectrum (Fig. S4a, ESI†) shows that the Co-VN/NC network consists of V, N and C elements, and an obvious peak of Co 2p can be observed, clarifying the successful Co element doping in the VN nanocrystals.16 The high-resolution XPS spectra of Co 2p in Fig. 3c show two peaks at 796.4 and 781.2 eV, which can be attributed to the Co 2p1/2 and Co 2p3/2 doublet, respectively. The deconvoluted XPS spectrum of V 2p in Fig. S4b (ESI†) indicates the presence of V–N (514.1 eV, 522.3 eV), V–N–O (515.7 eV, 522.4 eV) and V–O (516.9 eV, 524.7 eV) bonds, and the oxygen-containing functional groups on the surface of Co-VN could play roles in anchoring LiPSs.32 The N1s spectrum can be deconvoluted into four peaks, as shown in Fig. S4c (ESI†), and the characteristic peaks at 397.3 eV, 398.5 eV, 400.3 eV and 401.4 eV can be attributed to V-N, pyridine N, pyrrolic N, and graphite N, respectively.33 By carefully fitting the C 1s spectrum (Fig. S4d, ESI†), three prominent peaks at 284.7 eV, 285.8 eV and 288.3 eV can be assigned to the C–C, C–N and CO bonds, respectively.34 The presence of C–N bonds changed the nonpolar surfaces of graphitic carbon and thus enhanced their affinity to LiPSs.35
In addition, the Raman scattering spectra (Fig. 3d) were obtained to confirm the degree of graphitization for the Co-VN/NC, VN/NC and NC, and two typical peaks around 1340 (D-band) and 1590 cm−1 (G-band) indicate the existence of disordered carbon and graphitic carbon, respectively.36,37 The intensity ratio (ID/IG) of Co-VN/NC, VN/NC and NC was characterized as 0.934, 0.956 and 0.866, respectively, indicating a high graphitization degree, which can enhance the electrical conductivity of the composites. The pore structure characteristics of the 3D Co-VN/NC framework were investigated using N2 adsorption–desorption measurements, as shown in Fig. 3e, and the corresponding specific surface area for the prepared sample is 119 m2 g−1. The type IV isotherm and the pore size distribution together imply the coexistence of micro-, meso-, and macropores in the Co-VN/NC.22,38 The micropores afford higher adsorption energy for physically restricting LiPSs in the cathode, the existence of mesopores provides an appropriate length of ionic/electric diffusion path for LiPS conversion, and the macropores expose lots of Co-VN particles and accommodate the high sulfur loading of the cathode.39 The thermogravimetric analysis (TGA) profile of Co-VN/NC/S in Fig. 3f shows that the sulfur content is about 79.8 wt%, and the corresponding XRD patterns of the porous materials after sulfur was incorporated are shown in Fig. S5a (ESI†), which display typical peaks indexed to S8 (JCPDS: 08-0247).40 Meanwhile, the fact that sulfur was uniformly distributed on the surface of the 3D Co-VN/NC framework can be verified by SEM (Figure S5b and c, ESI†).
The strong chemical adsorption of the 3D Co-VN/NC framework to LiPSs was verified by adding 5 mg of the host material to 5 mM Li2S6 solution (3 ml). As shown in Fig. 4a, the brown polysulfide solution containing Co-VN/NC became nearly colorless after 2 h, while the color of the VN/NC sample solutions just lightened slightly and the solution with NC still kept a brown color, suggesting that the anchoring capability of VN has been enhanced after cobalt doping. Moreover, ultraviolet-visible (UV-Vis) adsorption tests further verified the role of cobalt doping in polysulfide entrapment. It is clear that the absorbance peak of the solution with Co-VN/NC almost disappears in the 400–500 nm range, which dramatically confirms that the Co-VN/NC framework possesses excellent adsorption capability toward LiPSs due to the strong polar nature of the Co dopants.41 XPS spectra of Co-VN/NC after soaking in Li2S6 solutions were collected (Fig. 4b). The Co 2p1/2 and 2p3/2 peaks of the Co-VN/NC/Li2S6 showed a significant negative shift, indicating that the strong interaction between LiPSs and Co increased the electron density at the metal center, which implies the formation of Co–S bonds.42
To further explore the in-depth effect of Co doping of VN to achieve efficient polysulfide trapping and redox kinetics, density functional theory (DFT) calculations were carried out. Fig. 4c shows the partial densities of states (PDOS) for V, N and Co atoms of VN and Co-VN, and there is no energy gap near to the Fermi level after cobalt doping, which indicates the metallic nature of Co-VN.33 Impressively, the Co-VN exhibited a higher V d band center (−0.730) compared with that of VN (−0.768), suggesting that the doped cobalt embellishes the electronic structure of VN and enhances the adsorption ability toward polysulfides.43 And the d band center of Co-VN with different Co doping ratios was also calculated, and the calculation results display that the d band center was increased first and then decreased when subjected to increasing Co doping levels (Fig. S6, ESI†). Then, the optimal geometric structures of Li2Sn (n = 1, 2, 4, 6, 8) adsorbed on the Co-VN surfaces are provided in Fig. 4e, and the formed Co–S bond indicates that the Co atom can adsorb the polysulfides.44 The adsorption energy (Ea) calculation results are indicated in Fig. 4d, and the Ea values for Co-VN with Li2S, Li2S2, Li2S4, Li2S6, and Li2S8 species are −2.29, −2.69, −2.47, −2.69 and −2.68 eV, respectively, which are obviously higher than those of VN (our previous work).40 This is due to the d electron transfer from Co ions to VN; the changing coordination environment of VN causes more active sites to be exposed, which promotes the interactions between electron-rich VN and LiPSs as well as sulfur redox kinetics.45 In addition, the separators and lithium anodes in different batteries after 50 cycles were disassembled. As shown in Fig. 4f1–2, there are apparent yellow LiPSs on the separator of the NC and VN/NC cathode, and the surfaces of the corresponding lithium foils were corroded, indicating a certain amount of LiPS shuttling to the anode.28,46 As seen from Fig. 4f3, the 3D Co-VN/NC framework can effectively relieve the shuttle effect, and these results further strongly demonstrate the enhanced trapping capability of VN after Co doping.
Apart from the effective adsorption effect, we also investigated the electrocatalytic reaction kinetics for cobalt-doped VN, and the lithium-ion diffusion coefficient (DLi) was analyzed through cyclic voltammetry (CV) testing of the Co-VN/NC/S, VN/NC/S and NC/S cathodes (Fig. 5a and Fig. S7a, b, ESI†). The DLi values for the different electrodes were calculated according to the Randles–Sevcik equation:
Ipeak = (2.69 × 105)n1.5ADLi0.5v0.5CLi | (3) |
To further verify the electrocatalytic effects, the contribution of cobalt doping to the improved conversion kinetics of LiPSs was confirmed by the symmetric cell tests. As illustrated in Fig. 5e, the voltammogram of Co-VN/NC without Li2S6 shows negligible capacitance, and the NC electrode shows only a pair of broad redox peaks with a large peak separation, indicating the poor reaction kinetics. In contrast, the Co-VN/NC and VN/NC electrodes with Li2S6 both clearly display three pairs of redox peaks, and the peaks around −0.05/0.05V, −0.27/0.27V and −0.07/0.07V represent the reversible stepwise redox reactions of Li2S6 Li2S4, Li2S4 Li2S2/Li2S, and S8 Li2S6, respectively.49,50 Moreover, the Co-VN/NC cell exhibits smaller peak separation and higher current intensity relative to VN/NC, implying the significantly boosted conversion kinetics between LiPSs and Li2S, which is ascribed to the catalytic effects of the dopant cobalt element. To gain insight into the catalytic processes of the 3D Co-VN/NC framework for polysulfide conversion, the calculation of the Li ion diffusion pathways on both the Co-VN and VN surfaces was further implemented and the results are shown in Fig. 5f. The energy barrier of the Li ion along the diffusion coordinate on Co-VN is 0.92 eV, which is lower than that on VN (1.01 eV), reflecting the faster interfacial ion transfer dynamics of VN after cobalt doping, which can dramatically facilitate the reversible conversion of LiPSs during oxidation–reduction processes.51,52 And the diffusion pathways of Li ions on Co-VN and VN surfaces are displayed in Fig. 5f and Fig. S8 (ESI†), respectively. The nucleation experiments of Li2S on the Co-VN/NC, VN/NC and NC catalysts further demonstrate the enhanced LiPS conversion (Fig. 5g–i).24,53 According to Faraday's law, Co-VN/NC shows the largest capacity of Li2S precipitation (240.8 mA h g−1), which is much higher than that of VN/NC (160.7 mA h g−1) and NC (97.7 mA h g−1), implying that Co-VN/NC can significantly promote the reduction of LiPSs. Moreover, the nucleation experiments of Li2S on Co-VN/NC with different Co doping contents were also studied, the results show that the activity of Li2S precipitation was the highest when the Co doping content in Co-VN was 3 at% (Fig. S9a–d, ESI†).
The electrochemical properties of Co-VN/NC, VN/NC and NC as the sulfur host were systematically evaluated in the following research. Fig. 6a displays the typical CV curves of different electrodes between 1.7 and 2.8 V at a sweep rate of 0.1 mV s−1. A pair of reduction peaks are observed during the discharge process, assigned to the reduction of sulfur to long-chain LiPSs at higher voltage and the formation of insoluble Li2S2/Li2S at a lower voltage, respectively.54 Besides, two overlapped oxidation peaks during the charging process stand for the conversions from Li2S2/Li2S to lithium polysulfides and finally to sulfur.55 Compared to the VN/NC and NC electrodes, the CV curve of the Co-VN/NC exhibits a positive shift of the reduction peaks and a negative shift of the oxidation peak, representing the less polarization and benign reversibility.4 In other words, due to the synergistic electrocatalytic effects of cobalt doping VN nanocrystals, the Co-VN/NC electrodes exhibited the sharpest peak currents and smallest polarization compared to the VN/NC and NC. At the same time, the charge–discharge voltage plots of different cathodes are shown in Fig. 6b. Compared to the initial capacity of the cathodes with VN/NC (1219 mA h g−1) and NC (1111 mA h g−1), the Co-VN/NC cathode exhibits much larger capacity of 1521 mA h g−1, and much higher sulfur utilization of 90.8% (based on the theoretical value of sulfur, 1675 mA h g-1).56 Additionally, we calculated the polarization potential (ΔE) between the oxidation and reduction plateau in Fig. 6c, and the Co-VN/NC cathode shows a smaller plateau voltage gap (ΔE = 145 mV) than the VN/NC (ΔE = 150 mV) and NC (ΔE = 158 mV) cathodes, representing higher reversibility and more efficient conversion kinetics of sulfur redox reactions.57 The discharge capacity ratio of low and high voltage plateaus (Q2/Q1) was calculated to explain the kinetics of the reduction process as illustrated in Fig. 6c. It is clear that the Q2/Q1 ratio of the Co-VN/NC cathode (2.54) is much higher than that of VN/NC (1.94) and NC (1.76), further revealing that the Co-VN electrocatalyst can effectively propel the reaction kinetics of liquid–solid conversion.58
The rate capabilities of the cells with Co-VN/NC, VN/NC and NC cathodes were evaluated from 0.1 to 4 C and returning to 0.2 C (Fig. 6d). Compared with other cathodes, the Co-VN/NC cathode displays superior capacities of 1172, and 688 mA h g−1 at 0.5 and 4 C, respectively, and achieves a high capacity of 1229 mA h g−1 even when the current density returns to 0.2 C. Fig. 6e exhibits the galvanostatic charge and discharge curves of the Co-VN/NC cathode at different current rates, and the discharge profiles distinctly show two-reductive-plateaus even though the current density is at 4 C, which further demonstrates that the Co-VN/NC electrocatalyst achieves excellent reaction kinetics. After the rate tests, the comparative cycling stability of these cells was measured at 0.5 C (Fig. 6f). After 300 cycles, the Co-VN/NC cathode retained a high reversible capacity of 876 mA h g−1 with a capacity retention of 86.5%. In comparison, the VN/NC and NC cathodes present discharge capacities of 478 and 225 mA h g−1 after 300 cycles, respectively. Fig. 6g demonstrates the long-term cycling performance of the Co-VN/NC cathode at 2 C over 1000 cycles, delivering a remarkable capacity retention of ∼490 mA h g−1 with a low capacity decay of 0.043% for each cycle, and a Coulombic efficiency of nearly 100% in all the cycles. In order to evaluate the commercialized applications of Co-VN/NC, Li–S batteries with high sulfur loading were investigated (4.83 mg cm−2). As displayed in Fig. 6h, the cell delivers an excellent initial area-specific capacity of 4.98 mA h cm−2 and retains 4.70 mA h cm−2 (94.3%) after 100 cycles at 0.2 C, which is higher than that of commercial lithium-ion batteries (4.0 mA h cm−2).59,60 Compared with other previously reported host materials for Li–S batteries (Table S2, ESI†), the electrochemical performance of the 3D Co-VN/NC cathode exceeds most relevant studies, indicating the outstanding advantage of cobalt-doped VN nanocrystals as high-performance hosts for a lithium–sulfur battery.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1nh00512j |
‡ Yang Lu and Menglong Zhao contributed equally to this work. |