Ayusie
Goyal
a,
Trinh Hai
Binh
b,
Labham
Singh
a,
Pragya
Arora
a,
Anamika
Yadav
a,
Chung-Li
Dong
*b,
Baghendra
Singh
*a and
Apparao
Draksharapu
*a
aSouthern Laboratories - 208A, Department of Chemistry, Indian Institute of Technology Kanpur, Kanpur-208016, India. E-mail: appud@iitk.ac.in; baghendras@iitk.ac.in
bDepartment of Physics, Tamkang University, New Taipei City, Taiwan. E-mail: cldong@mail.tku.edu.tw
First published on 30th December 2025
Identification of the active sites responsible for both the oxygen evolution reaction (OER) and the iodide oxidation reaction (IOR) is critical for the rational design of high-performance catalysts. However, active sites for the IOR have not been previously explored to the best of our knowledge. Herein, we investigate the active sites of the OER and IOR on a benzoate-coordinated NiCo-hydroxide (BZ-NiCo-H) catalyst. Spectroscopic studies reveal that benzoate coordination modulates the electronic and coordination environment, facilitating the generation of high-valent metal species. BZ-NiCo-H exhibited excellent catalytic activity, delivering 100 mA cm−2 at 1.42 V vs. RHE potential for the IOR and 1.63 V vs. RHE potential for the OER. In situ Raman spectroscopy coupled with electrochemical analyses identifies Ni4+ in γ-Ni(O)OH as the OER active site, whereas Ni3+ in β-Ni(O)OH functions as the active site for the IOR. Mechanistic investigations demonstrate that benzoate coordination activates lattice oxygen, enabling the OER to proceed via a lattice oxygen mechanism (LOM). Furthermore, in situ electrochemical impedance spectroscopy and kinetic studies show that benzoate coordination significantly enhances charge transfer and lowers kinetic barriers for both reactions. These findings elucidate the distinct active sites for the OER and IOR, highlighting the beneficial role of organic ligand coordination in tuning catalytic performance.
Among the various AORs, the IOR has recently gained attention as a promising alternative to the OER, primarily due to its ability to produce high-value added iodate (IO3−) (Fig. 1a and b).4,5 Iodate is a commercially important compound with diverse applications in the pharmaceutical industry, iodized salt production, and analytical chemistry, and as an oxidizing agent at both laboratory and industrial levels.6,7 Despite its potential, the IOR has remained largely underexplored compared to other AORs such as HzOR, UOR, GOR, AmOR, and AlOR.8,9 Only a limited number of studies have explored electrocatalysts for IOR-assisted water electrolysis, and to the best of our knowledge, none have demonstrated high current densities more than 200 mA cm−2, an important threshold for practical applications.10,11
Electrocatalysts based on nickel have recently been identified as some of the best materials for promoting the OER.12–14 During the OER, Ni2+ sites undergo anodic oxidation to high-valent Ni oxyhydroxide phase, which are generally accepted as the true catalytically active states.15–17 Therefore, facilitating the generation of such high-valent metal oxyhydroxides is expected to accelerate the overall OER kinetics. Over the last few decades, considerable efforts have been devoted to identify the real active sites for the OER in Ni-based catalysts.18–23
In contrast, the design of efficient electrocatalysts for the IOR has recently begun to attract attention. A few materials, including MoS2–FeS2,24 CoP,25 and CoFe-NC,26 have been investigated as IOR catalysts, and our group has recently reported a strain-engineered V–Fe(O)OH system for this purpose.27 Nevertheless, the precise identification of the catalytically active sites in the Ni-based catalysts for IOR remains underexplored, and the reported catalysts still suffer from limited activity and stability. These challenges highlight the urgent need to uncover the underlying reaction mechanism and pinpoint the true active sites, which would provide a rational basis for designing highly efficient and durable IOR electrocatalysts.
To address this challenge, we have reported a benzoate-coordinated NiCo-hydroxide (BZ-NiCo-H) that exhibited efficient activity for both the OER and IOR (Fig. 1c). X-ray absorption spectroscopy (XAS) validated that benzoate coordination optimized orbital overlap and modified both the electronic feature and coordination environment, thereby facilitating easier access to high-valent metal sites. The increased interlayer spacing provided the facile diffusion of electrolyte and more accessible active sites. For the IOR, BZ-NiCo-H achieved a remarkable 100 mA cm−2 at just 1.42 V vs. RHE potential, while for the OER, it required 1.63 V vs. RHE potential to deliver the same current density. The superiority of this system became even more apparent when integrated into a tandem IOR-assisted water electrolysis system, where it achieved 100 mA cm−2 current density at a cell voltage of 1.92 V, a dramatic reduction from the 2.15 V, typically needed for conventional water splitting. This tandem configuration enhanced energy efficiency by 57%.
Mechanistic studies revealed that benzoate coordination induced a distinct reaction pathway. Interestingly, BZ-NiCo-H showed a LOM pathway governed by proton-decoupled electron transfer (PDET). In situ Raman analysis demonstrated that γ-Ni(O)OH (Ni4+) was the main active phase for the OER, while β-Ni(O)OH (Ni3+) served as the active phase for the IOR in BZ-NiCo-H. Arrhenius kinetic analysis and in situ electrochemical impedance spectroscopy (EIS) suggested that benzoate coordination significantly enhanced charge transfer kinetics and reduced activation energy barriers. These effects collectively contributed to the accelerated reaction rates observed for the OER and IOR. These findings underscore the promise of linker-coordinated hydroxides for sustainable value-added electrochemical transformations.
Powder X-ray diffraction (PXRD) patterns further validated the phase composition of the synthesized materials. The diffraction peaks in BZ-NiCo-H were observed at 5.93°, 11.82°, and 17.70°, corresponding to the (001), (002), and (003) planes of the Ni(OH)(C6H5COO) H2O phase, matching with JCPDS No. 42-1836 (Fig. S2). Additionally, the diffraction peaks in NiCo-H were observed at 19.78°, 33.61°, and 39.09°, attributed to the (001), (100), and (101) planes of the β-Ni(OH)2 phase (JCPDS No. 14-0177) (Fig. S2). The peak at 5.93° in BZ-NiCo-H corresponded to the d-value of 1.48 nm, which indicated that the linker coordination increased the interlayer spacing.30,31
The oxidation states of the elements in BZ-NiCo-H and NiCo-H were examined using X-ray photoelectron spectroscopy (XPS). The Ni 2p spectrum of BZ-NiCo-H exhibited peaks at 856.23 eV and 873.88 eV corresponding to Ni 2p3/2 and Ni 2p1/2, respectively (Fig. 2a).29,31–33 The peak for Ni2+ was recorded at 856.38 eV. In BZ-NiCo-H, the Ni 2p3/2 peak exhibited a positive shift of 0.67 eV relative to NiCo-H, indicating the existence of high-valent Ni sites in BZ-NiCo-H. The Co 2p spectrum of BZ-NiCo-H revealed the peaks at 781.37 eV and 796.55 eV, assigned to Co 2p3/2 and Co 2p1/2, respectively (Fig. 2b).31,34–36 The signal at 780.77 eV was attributed to the Co2+ species. The signal associated with Co 2p3/2 of BZ-NiCo-H exhibited a positive binding energy shift of 0.50 eV, relative to NiCo-H. The positive shift indicated the presence of high-valent Co sites in BZ-NiCo-H.
Furthermore, the O 1s spectrum of BZ-NiCo-H revealed two signals for surface –OH groups at 531.86 eV and metal–oxygen bond at 529.46 eV (Fig. S3).37,38 The peak of the –OH group in O 1s XPS of NiCo–H was observed at a binding energy of 531.2 eV, whereas in the case of BZ-NiCo-H it was seen at 531.86 eV, reflecting a negative shift of 0.84 eV in NiCo-H compared to BZ-NiCo-H (Fig. S3). The XPS study established that linker coordination altered the coordination and electronic features of BZ-NiCo-H.
The coordination and electronic properties of the catalysts were thoroughly investigated using X-ray absorption spectroscopy (XAS) studies. NiCo-H and BZ-NiCo-H exhibited distinct coordination and electronic characteristics, particularly in terms of metal oxidation states and coordination environments. The Ni K-edge XANES spectra of both NiCo-H and BZ-NiCo-H displayed a prominent absorption peak (∼8350 eV), comparable to that of the NiO standard, indicating the presence of the Ni2+ state, coordinated in an octahedral environment (Fig. 2c).39,40 The pre-edge features of NiCo-H and BZ-NiCo-H observed at around 8335 eV were attributed to metallic Ni, arising from the underlying Ni foam.
Notably, the main absorption peak of BZ-NiCo-H exhibited a higher intensity than that of NiCo-H, implying an increased oxidation state of Ni, associated with low-spin Ni3+ in BZ-NiCo-H. In BZ-NiCo-H, the low-spin Ni3+ species exhibited an e1g configuration, inducing a Jahn–Teller distortion within the catalyst lattice. Such structural distortion promotes favorable adsorption–desorption of reaction intermediates, thereby enhancing the overall catalytic activity. For the Co K-edge XANES, both BZ-NiCo-H and NiCo-H displayed characteristic features indicative of Co2+ in an octahedral coordination environment, closely resembling the CoO reference (Fig. 2d).41,42 Moreover, the absorption edge positions for both catalysts were significantly higher and closely aligned with CoO, further confirming that Co predominantly exists as Co2+. Additionally, the Co K-edge XANES spectra displayed a pre-edge feature at ∼7710 eV, with BZ-NiCo-H showing a more intense pre-edge peak than NiCo-H (Fig. 2d inset). This was attributable to increased Co 3d-4p orbital mixing, suggesting the greater degree of structural distortion in BZ-NiCo-H. Furthermore, the observed shift of the main absorption peak to higher energy in BZ-NiCo-H relative to NiCo-H validated an elevated oxidation state of Co, reflecting the changes in the coordination environment due to the linker coordination.
The Ni R-space profile of NiCo-H exhibited two distinct peaks located at approximately 1.50 Å and 2.49 Å, corroborated with Ni–O and Ni–Ni/Co coordination, respectively (Fig. 2e).43,44 A noticeable shortening in the distance of the Ni–O bond was observed in BZ-NiCo-H compared to NiCo-H. This bond contraction was associated with an increased oxidation state of Ni in BZ-NiCo-H. The increased peak intensity of the Ni-O shell in BZ-NiCo-H compared to NiCo-H suggested a higher coordination number around the Ni atom, which could be due to the stronger coordination effect induced by the benzoate linker. The above observation further indicated that linker coordination changed the electronic structure of Ni sites.
To further explore the structural differences, the Co R-space profile was analysed. In the profile, two primary features at around 1.45 Å and 2.83 Å were associated with the Co–O and Co–Co/Ni coordination shells, respectively (Fig. 2f).45,46 For BZ-NiCo-H, the bond distance in the Co–O first shell was reduced compared to the NiCo-H. This bond contraction was attributed to the coordination of the benzoate linker, which increased the crystal field strength and stabilized the low-spin Co3+ state, as also supported by the main absorption feature in Fig. 2d. In addition, the decreased peak intensity of the Co–O shell in BZ-NiCo-H reflected local structural distortion, consistent with the enhanced pre-edge peak intensity observed in the XANES spectra.
The average oxidation state of Ni in BZ-NiCo-H and NiCo-H was estimated by establishing a linear relationship between the first derivative peak energy and the nominal oxidation states of Ni standard samples. Based on the analytical results, the average Ni oxidation states in BZ-NiCo-H was estimated to be +2.60, which was higher than that in NiCo-H (+2.23) (Fig. S4). Correspondingly, the average oxidation state of Co was also derived from the Co K-edge XANES using the same first derivative approach. The results indicated that the Co average oxidation state in BZ-NiCo-H (+2.31) was higher than that in NiCo-H (+2.09) (Fig. S4). The XAS analysis clearly demonstrated that benzoate linker coordination promoted the facile access of high-valent Ni and Co sites, to improve the anodic oxidation activity.
Transmission electron microscopy (TEM) and scanning electron microscopy (SEM) were used to analyze the surface features of the synthesized materials. SEM images of BZ-NiCo-H revealed the growth of long nanowires across the nickel foam, while NiCo-H exhibited nanosheet-like morphology (Fig. S5). The TEM analysis of BZ-NiCo-H further confirms the nanowire morphology, while HR-TEM displayed a stripe spacing of 1.25 nm, suggesting the microporous structure (Fig. 3a and b).47 These findings suggested that the coordination of benzoate linkers led to a structural reorganization of the material to form 1D nanowires, which had micropores facilitating the electrolyte diffusion. The existence of Ni, Co, O, and C in BZ-NiCo-H and Ni, Co, and O in NiCo-H was validated by energy-dispersive X-ray spectroscopy (EDX) and associated elemental mapping, demonstrating their elemental composition (Fig. S6–S9).
To further elucidate the underlying mechanism of the OER, the pH-dependence of OER activity was evaluated at different pH values (13.50, 13.68, 13.80, and 13.90) (Fig. S11).48–50 Notably, BZ-NiCo-H exhibited a larger sensitivity to pH changes compared to NiCo-H. The correlation between current density and pH provides critical insight into the involvement of protons in the OER when referenced against the RHE scale. The evaluated ρRHE value for BZ-NiCo-H was 0.75, substantially lower than that of NiCo-H (0.52) (Fig. 4b).
A ρRHE value close to 1 indicates that the OER activity of the catalyst is highly influenced by pH. This suggests that BZ-NiCo-H likely operated via the lattice oxygen mechanism (LOM), where proton and electron transfers occurred in a decoupled manner. In comparison, NiCo-H displayed a lower ρRHE and a weaker pH dependence, pointing toward the adsorbate evolution mechanism (AEM).
Further mechanistic distinction was achieved using tetramethylammonium (TMA+) cations as mechanistic probes. In the LOM pathway, peroxo intermediates interact with TMA+, leading to a decline in OER activity (Fig. S12).48–50 NiCo-H exhibited minimal variation in activity in the presence of TMA+, corroborating an AEM-type mechanism. In contrast, BZ-NiCo-H showed a marked decrease in catalytic performance in TMAOH, indicating significant interaction between TMA+ and reactive peroxo intermediates, and thus validating its LOM behavior. These results collectively confirmed that benzoate coordination in BZ-NiCo-H modulated the OER pathway, favoring LOM.
To further explore the pH dependence of OER thermodynamics, Pourbaix diagram was constructed at a low current density (10 mA cm−2) (Fig. S13).50,51 The slope derived for BZ-NiCo-H was 118.3 mV pH−1, while NiCo-H exhibited a slope of 105.5 mV pH−1. According to the Nernst equation, a slope of ∼59 mV pH−1 corresponds to a 1
:
1H+/e− stoichiometry, whereas a slope near 118 mV pH−1 implies a 2H+/2e− transfer process. Thus, the 118.3 mV pH−1 slope for BZ-NiCo-H suggested the involvement of a two-proton–two electron transfer.
To demonstrate the superior OER kinetics of BZ-NiCo-H relative to its counterpart NiCo-H, a series of temperature-dependent electrochemical measurements were performed (Fig. S14).52–54 LSV was conducted over a range of temperatures, revealing a consistent enhancement in OER activity as the temperature increased, an expected outcome given the thermally activated nature of electrochemical reactions.
To quantitatively evaluate the temperature effect on reaction kinetics, the LSV data were analyzed using the Arrhenius equation.52–54 The activation energies (Ea) for the OER were extracted by plotting the logarithm of current density against the reciprocal of temperature at a constant potential. BZ-NiCo-H possessed a significantly smaller activation energy of 14.01 kJ mol−1, compared to NiCo-H (18.68 kJ mol−1), confirming the enhanced kinetic favorability of the benzoate-coordinated catalyst (Fig. 4c). The reduced activation energy reflects a lower enthalpic barrier for the OER, which is attributed to the electronic modulation introduced by linker coordination.
To investigate how benzoate coordination into NiCo-H enhanced catalytic activity and to evaluate the interfacial catalytic dynamics, in situ electrochemical impedance spectroscopy was performed across a range of applied potentials (Fig. 5a, b and S15).52–54 The Bode analysis revealed that different frequency domains corresponded to distinct electrochemical processes: high-frequency responses related to the activation of catalytic sites, while low-frequency signals corresponded to faradaic processes associated with the OER. Compared to NiCo-H, BZ-NiCo-H displayed a lower phase angle in the high-frequency region, indicating more effective activation of the catalyst to create high-valent metal sites (Fig. 5a and b).
With increasing applied potential, the low-frequency phase angle decreased. For BZ-NiCo-H, the Bode phase plots showed the onset of the OER at approximately 1.50 V vs. RHE, which was lower than the 1.55 V required for NiCo-H, reflecting a reduced energy barrier for reaction initiation (Fig. 5a and b).52–54 The onset potential of both the catalysts was also corroborated with the LSV profiles. This analysis further confirmed that benzoate coordination facilitated easier accessibility to Ni3+/Ni4+ sites at lower potentials, thereby enabling the OER to be initiated at a reduced onset potential. Beyond the onset, BZ-NiCo-H exhibited a steeper drop in low-frequency phase angle, signifying faster OER kinetics.
BZ-NiCo-H also demonstrated a lower Rct (2.81 Ω) compared to NiCo-H (4.48 Ω) at 1.55 V vs. RHE, implying faster charge transfer properties in BZ-NiCo-H (Fig. S15). Additionally, the admittance at the lowest frequency, linked to long-range charge mobility, was higher for BZ-NiCo-H (0.19 S) than NiCo-H (0.16 S), confirming improved charge transport (Fig. S15). Analysis of charge-transfer resistance (Rct) and phase angle beyond the OER onset further validated the advantage of benzoate coordination. BZ-NiCo-H exhibited markedly lower Rct values and reduced phase angles, highlighting its superior charge-transfer efficiency and faster reaction kinetics relative to NiCo-H, underscoring the beneficial role of benzoate coordination in boosting electrocatalytic performance.
To validate the enhanced IOR kinetics of BZ-NiCo-H compared to the unmodified NiCo-H, temperature-dependent electrochemical analyses were carried out (Fig. S17).52–54 LSV was performed across various temperatures, consistently showing improved IOR performance with rising temperature, an outcome aligned with the thermally driven nature of electrochemical processes. To quantify the influence of temperature on reaction kinetics, the LSV results were further interpreted using the Arrhenius equations.52–54 BZ-NiCo-H demonstrated a significantly smaller activation energy of 6.71 kJ mol−1 than NiCo-H (11.97 kJ mol−1), indicating superior IOR kinetics (Fig. 4d). This reduction in Ea suggested that benzoate functionalization effectively tuned the electronic structure of the catalyst, facilitating more favorable reaction kinetics.
In situ EIS was employed to gain further insights into the IOR using both the synthesized catalysts (Fig. 5c, d and S18).52–54 The obtained Bode spectra revealed two distinct electrochemical processes. The low-frequency domain was attributed to the IOR, while the high-frequency region corresponded to the intrinsic electrochemical reconstruction dynamics to generate catalytically active phases. The pronounced variation and reduced phase angle with increasing potential in the high-frequency region suggested that BZ-NiCo-H underwent a more rapid reconstruction process to generate the active phase compared to NiCo-H (Fig. 5c and d). Furthermore, in the low-frequency region, BZ-NiCo-H exhibited a lower phase angle than NiCo-H for the IOR process, suggesting that BZ-NiCo-H enabled more efficient charge transfer and faster reaction kinetics during the IOR. Compared with the OER, the decrease in phase angle within the low-frequency region during the IOR indicated a lower onset potential and more favorable reaction kinetics for the IOR relative to the OER in both catalysts.
To reach a current density of 100 mA cm−2, a cell voltage of 2.15 V was required for overall water electrolysis, whereas IOR-assisted water electrolysis achieved the same current density at a lower voltage of 1.92 V, demonstrating improved overall cell efficiency (Fig. S19). This approach enhanced energy efficiency by 57%, lowering the energy consumption from 4.90 kWh m−3 H2 of conventional water electrolysis to 2.08 kWh m−3 H2 of IOR-assisted water electrolysis (Fig. S20).27
A key observation lies in the distinct differences in the δ(Ni–O) to ν(Ni–O) intensity ratio (denoted as Iδ/ν) in the catalyst, which reflect variations in the active catalyst phase.60–63 Typically, Ni(O)OH can crystallize in β or γ phases, with γ-Ni(O)OH, exhibiting a comparatively weaker ν(Ni–O) band and a higher Iδ/ν, due to its more open, disordered framework. BZ-NiCo-H showed a higher Iδ/ν value at 1.5 and 1.6 V vs. RHE, suggesting γ-Ni(O)OH as the active phase for the OER.60–63 Literature reports indicate that γ-Ni(O)OH is enriched with highly oxidized Ni4+ species, corresponding to an average Ni oxidation state of about +3.7.60–63 This analysis indicates Ni4+ in the γ-Ni(O)OH phase as the active site for the OER. In an alkaline electrolyte, γ-Ni(O)OH generally promotes O–O coupling via producing a NiOO− intermediate on Ni4+, characteristic of the LOM pathway.60–63 This characteristic Raman band of NiOO− was observed at 1060 cm−1, indicating a LOM pathway for the OER, which further supported the pH-dependent and TMAOH experiments.64
Similarly, in situ Raman spectroscopy was conducted to determine whether Ni3+ or Ni4+ species participates in the IOR process (Fig. 6b). Similar to the OER, two distinct Raman bands characteristic of the β-Ni(OH)2 phase appeared at 450 and 530 cm−1 from 1.1 V to 1.3 V vs. RHE.55–59 As the potential increased to 1.4 V, these bands gradually shifted to 462 and 543 cm−1, corresponding to the Eg bending mode and the A1g stretching mode of Ni(O)OH, respectively.60–63Furthermore, the intensity of these bands increased as the potential was increased up to 1.6 V vs. RHE. Interestingly, the Iδ/ν ratio was observed to be 0.95 and 0.92 at 1.50 V and 1.60 V vs. RHE, respectively, indicating preferential creation of β-Ni(O)OH with dominant Ni3+ sites as the active phase for the IOR.60–63 Additionally, at the potential of 1.4 V vs. RHE, where β-Ni(O)OH was generated, a new vibrational band emerged at 757 cm−1, attributed to the surface adsorbed IO3−.65–67 As the β-Ni(O)OH bands intensified with an increase in potential, the IO3− band also enhanced , indicating that Ni3+ species played a dominant role in catalyzing the oxidation of iodide to IO3−.
Furthermore, CV analysis revealed a sequential oxidation of Ni2+ [Ni(OH)2] to Ni3+ [Ni(O)OH] during anodic scanning in 1.0 M KOH.68 Additionally, the disappearance of the Ni2+/Ni3+ anodic peak in CV after KI addition supports the consumption of Ni3+ during the IOR (Fig. 6c). Interaction of iodide ions with β-Ni(O)OH involving Ni3+ as the true active sites was validated by chronoamperometry (Fig. 6d). Upon the addition of KI, a sharp current increase (∼150 mA cm−2 from ∼14 mA cm−2) was observed, indicating an immediate redox interaction between I− and Ni(O)OH. In situ Raman spectroscopy and CV studies unequivocally identified Ni3+ as the active site facilitating the IOR, while Ni4+ was determined to be the catalytically active species for the OER (Fig. 6e).
To elucidate the active sites in NiCo-H, in situ Raman spectroscopy was performed. At a lower potential of 1.3 and 1.4 V vs. RHE, no band was observed while at the potential of 1.5 and 1.6 V vs. RHE, two characteristic bands at 471 and 556 cm−1 were detected, corresponding to the Eg bending mode [δ(Ni–O)] and A1g stretching mode [ν(Ni–O)] of the γ-Ni(O)OH phase, respectively (Fig. S21).60–63 This analysis indicates the generation of the γ-Ni(O)OH phase under an anodic potential, which acts as the key active site for the OER.
During the OER, Ni2+/Ni3+ species in Ni(OH)2/NiOOH undergo further oxidation to form highly oxidized Ni4+ [γ-Ni(O)OH]. It acts as the true active center for the OER, because its higher oxidation state facilitates lattice oxygen activation and deprotonation of OH intermediates. The formation of Ni4+ increases the electrophilicity of surface oxygen, promoting key OER steps such as M–O bond breaking, O–O coupling, and *OOH stabilization. Therefore, the presence of Ni4+ correlates with enhanced OER kinetics and lowers the overpotential. In contrast, the IOR operates at considerably lower potentials, where Ni2+ is oxidized only to Ni3+ [β-Ni(O)OH] but does not reach the Ni4+ [γ-Ni(O)OH]. The Ni3+/Ni2+ redox couple aligns well with the thermodynamics of iodide oxidation, making Ni3+ an effective redox mediator for the IOR. Ni3+ accepts electrons from iodide and is subsequently reduced back to Ni2+, allowing for rapid and reversible cycling of the catalyst and promoting the oxidation of iodide to iodate.