Open Access Article
Muralikrishna Sreeramareddygari
*a,
Jyothi Mannekote Shivanna
*b,
Zhoveta Yhobu
c,
S. Satyanarayana Reddy
d,
Mithran Somasundrum
ae,
Chatuporn Phanthongae,
Gurumurthy Hegde
fgi,
Patsamon Rijiravanich
ae and
Werasak Surareungchaiah
aSensor Technology Laboratory, Pilot Plant Development and Training Institute, King Mongkut's University of Technology Thonburi, Bangkhuntien-chaitalay Road, Thakam, Bangkok, 10150, Thailand. E-mail: sreerama.mur@kmutt.ac.th
bDepartment of Chemistry, Nitte Meenakshi Institute of Technology (NMIT), Nitte (Deemed to be University), Bengaluru, 560064, India. E-mail: jyothi0901@gmail.com
cDepartment of Chemical Sciences, Ariel University, Ariel 40 700, Israel
dDepartment of Physics, RV Institute of Technology and Management, Bengaluru, 560076, Karnataka, India
eIndustrial Sensor Technology Research Team, National Center for Genetic Engineering and Biotechnology, National Science and Technology Development Agency at KMUTT (Bangkhuntien Campus), Bangkok, 10150, Thailand
fDept of Chemistry, Christ University, Bangalore 560029, India
gCentre for Advanced Research and Development, Christ University, Bangalore 560029, India
hFaculty of Science, King Mongkut's University of Technology Thonburi, Pracha Uthit Rd, Thung Khru, Bangkok, 10140, Thailand
iCentre for Waste to Wealth Technology, Dayananda Sagar University, Devarakaggalahalli, Harohalli, Kanakapura Road, Bengaluru South Dt. – 562 112, India
First published on 27th May 2026
A novel screen-printing approach was employed to fabricate molybdenum disulfide (MoS2) based membranes using exfoliation-free solvothermally synthesized ink-like MoS2 gel and Whatman filter paper (WFP). Three membranes, MoS2-WFP-1, MoS2-WFP-2, and MoS2-WFP-3, were fabricated by varying the number of print coatings to tailor the hydrophobicity and mechanical integrity. Structural and morphological investigations were performed by X-ray Diffraction (XRD), X-ray Photoelectron Spectroscopy (XPS) and Field Emission Scanning Electron Microscopy (FE-SEM) analysis. The XPS results confirmed a well-adhered MoS2 layer with mixed 1T/2H phases that enhanced mechanical and thermal stability. The MoS2 incorporated membranes exhibited increased tensile strain, moderate water uptake (53–55%), and contact angles (104–118°) which increased with increasing coat number, demonstrating tunable surface wettability. In spite of reduced pure water flux, compared to bare filter paper, each coated membrane exhibited stable flux over a 60 min filtration period. The membranes efficiently removed the Congo red (∼90%), methylene blue (∼55%) and Cr(VI) (∼72%) under pH-dependent conditions. The pH-dependent removal arises from electrostatic interactions between the MoS2 surface and charged species, where protonation of the negatively charged MoS2 surface at acidic pH enhances the attraction of anionic contaminants (Congo red and Cr anions such as such as HCrO4− and Cr2O72−), while deprotonation at basic pH favors adsorption of cationic MB. The investigations confirm a simple, scalable and low-cost route for the fabrication of printable MoS2 membrane filters suitable for wastewater purification.
Molybdenum disulfide (MoS2)-based membranes have shown potential in water treatment applications, enhancing ion and molecular separation processes. Their unique physiochemical properties and fabrication techniques contribute to improved efficiency and reduced energy consumption in water purification, as highlighted in research over the last few years.8 MoS2 nanosheets possesses high surface area, good chemical and thermal stability and offer easy surface functionalization. The membranes fabricated using MoS2 nanosheets have exhibited superior water flux due to the hydrophilic nature of their edges and attain greater aqueous stability than that of graphene oxide or polymeric membranes.9 Different morphologies of MoS2, such as nanoplatelets, enhance performance by creating more water channels, achieving up to 93% removal of heavy metals like Mn2+ and Zn2+.10 Incorporating MoS2 into composite membranes can improve stability and separation efficiency, fostering advancements in membrane technology.8
The production of MoS2 composite membranes at near-atomic thickness presents technological hurdles, yet this is crucial for maximizing their water treatment efficiency.11 Chemical Vapour Deposition (CVD) and Atomic Layer Deposition (ALD) are widely employed measures to produce monolayer or sub-monolayer MoS2 thin films. These methods offer continuous, high uniform and large-area MoS2 nanosheets which are well aligned with the design and fabrication of MoS2 membranes. However, these methods are limited for wider applications due to their complicated fabrication process. This could substantially increase the membrane production costs and limit industrial scale applications.12 On the other hand, liquid exfoliation methods offer simple steps to produce MoS2 nanosheets. The resulting nanosheets can be functionalized with other molecules, or polymers, to regulate the structure and function of the MoS2. The resulting materials have been used for membrane fabrication through a simple vacuum filtration method.13 Nonetheless, these methods are also limited in practical use due to low scalability and the necessity of Li+ ions intercalation, which requires the use of hazardous solvents and an inert gas atmosphere.14 Electrochemical intercalation or micromechanical exfoliation methods are still facing challenges to scale up, due to low yields.15,16
Interfacial polymerization, involving reaction on a porous substrate,17 layer-by-layer assembly by sequential immersion cycles,18 electrospray polymerization,19 direct application of polymer on a support followed by phase inversion, and hybrid techniques such as electrospinning in combination with interfacial polymerization,19 dip or spin coating of the nanomaterials onto the pre-formed layers,20 are some of the other methods used for the fabrication of composite membranes to achieve thin but strong active layers on the supports. In one of our previous works, a scalable hydrothermal method was used for the production of defect rich MoS2 nanosheets, to develop highly stable functionalized membranes. The MoS2 membrane fabricated using pristine MoS2 nanosheets showed poor aqueous stability whereas the MoS2 nanosheets treated with trithiocyanuric acid (TTCA), prior to membrane fabrication through vacuum filtration, showed high aqueous stability and good heavy metal ion and molecular separation efficiency.21 The defect rich MoS2 nanosheets are functionalized and polymerized via thiol group containing TTCA, which greatly helped the strong adhesion onto the commercial Polyethersulfone (PES) membrane surface through hydrophobic π–π* stacking and electrostatic interactions between polythiocyanuric acid (PTCA) and PES. The fabricated membrane was able to remove dyes and heavy metals by ∼80%.
Screen-printing technology offers several advantages including easy tailoring, economical, control over thickness, reproducibility, a wide substrate scope and easier scalability.22 Screen-printing is a technology widely used in many industrial applications such as textiles, dye sensitized solar cells, silicon photovoltaics, printed electronics, sensors, snowboard graphics and medical devices.23–25 This technology is also used in the fabrication of membranes such as PVA-based charged mosaic membranes to evaluate ion transport properties,26 catalyst coated membranes in a proton exchange membrane fuel cells,27 and so on. MoS2 nanosheets are widely used for the fabrication of electrodes through screen printed technology to develop sensors, energy conversion and storage applications.28–30 However, the screen-printed method has been rarely reported in fabrication of membranes for water purification processes.
Most membrane filtration experiments demand an applied pressure for the filtration process, and some membranes, even with pressure, suffer from insufficient permeate flux. Hence, the present work proposes the fabrication of MoS2 membranes using ink-like MoS2 gel on a regular Whatman grade 1 filter paper (WFP) via screen-printing methods. A solvothermal method was used to synthesise a ink-like MoS2 gel suitable for screen-printing. This ink was screen-printed onto Whatman 1 filter papers to prepare MoS2-WFP-1, MoS2-WFP-2 and MoS2-WFP-3 membranes, using 1, 2, and 3 screen-printing passes respectively, of the MoS2 ink. The membranes were characterized using spectroscopic and microscopic methods. The water uptake, contact angle and mechanical properties of the fabricated membranes was investigated and the performance towards removal of dyes such as Congo red (CR), methylene blue (MB) and the heavy metal ion Cr(VI), at different pH conditions were also studied. This method enables the easy use of the fabricated membrane for water treatment applications, without the requirement of any specified membrane filtration units.
![]() | (1) |
This standardized gravimetric method ensures consistent evaluation of hydrophilic properties across different membrane formulations. The hydrophilic nature of the membrane surface was confirmed by contact angle measurements using a digital microscope and digital viewer.
The pure water flux (PWF) is another factor deciding the performance of the membrane. This was examined using a regular filtration unit of 1000 mL capacity, procured from Sigma Aldrich Pvt, Ltd. All water filtration experiments performed without applied pressure or without connection of vacuum pump. The volume of water permeated through membrane was measured every 10 min and the PWF (Jw, L m−2 h−1) was calculated from eqn (2), by measuring the time, t, (in h), volume, V, of water (in L) and membrane area, A, (in m2).
![]() | (2) |
![]() | (3) |
Although the hydrothermal route is simple, reproducible, and suitable for laboratory-scale production, its direct translation to large-scale manufacturing is limited by autoclave volume, batch processing, and the difficulty of maintaining uniform heat and mass transfer at higher volumes. Therefore, the present work should be regarded as a laboratory-scale demonstration of a potentially scalable route and further work on larger reactors or continuous synthesis would be required to establish industrial scalability.
Therefore, only the MoS2-WFP-1 was used for the spectroscopic and microscopic characterizations used to evaluate structural, chemical, thermal, and mechanical properties. The XRD patterns of WFP, MoS2-WFP-1 and MoS2 powder are provided in Fig. 1a and b. The WFP shows characteristic diffraction peaks at 2θ 14.6°, 16.2°, 22.38° and 33.8° which correspond to (110), (110), (200) and (004) diffraction planes of monolithic cellulose type I, respectively.34 MoS2 powder exhibits a dominant hexagonal 2H peak at 2θ 9.64° for reflecting (002) plane, which is corresponding to interlayer spacing of 0.92 nm. The downwards shift in (002) plane peak position from 14.13° to 9.64° demonstrates an enlarged interlayer spacing from 0.63 nm (JCPDS card 01-075-1539) to 0.92 nm, which was calculated based on Bragg's law (2d sin
θ = nλ), which clearly suggests an expansion of the layered structure compared to conventional 2H MoS2.35 Additional peaks at 2θ, 32.7° and 57° reflecting (100) and (110) planes confirm in-plane crystallinity and layered stacking. Additionally, the broad nature of the peaks demonstrates the amorphous nature of the synthesized ink. In the case of MoS2-WFP-1 (2θ at 9.64°), the absence of high-index diffraction peaks indicates short-range disorder within the nanocrystalline structure.36 This arises due nanoflake fragmentation during screen-printing. The absence of the same is also attributed to the very low concentration of MoS2 on the filter paper. The disordered configuration enhances active site density by exposing edge sulfur atoms, which are optimal for binding water contaminants like heavy metals. Also, the prominent cellulose peak and the less intense peaks of MoS2 in MoS2-WFP-1 confirms that the screen-printing process preserves the MoS2 crystal structure while integrating it with the substrate. BET analysis was performed to find out the specific surface area and pore volume of the MoS2. Fig. 1c displays the nitrogen adsorption–desorption isotherms of MoS2. According to the IUPAC classification, the solvothermally synthesized MoS2 exhibits a type-IV isotherm with a H3 type hysteresis loop, which indicates the characteristic of mesoporous materials. The attributed pores have presumably arisen due to the spaces between the cross-linked MoS2 nanosheets which yield a large specific surface area. The average pore diameter and specific surface area of the MoS2 are calculated to be 11.74 nm and 55.17 m2 g−1, respectively. However, the BET pore diameter represents the intrinsic mesoporosity of the MoS2 flakes, rather than the effective membrane filtration pore size, which is governed by the coated WFP architecture and interflake transport pathways.
![]() | ||
| Fig. 1 XRD patterns of (a) WFP, and MoS2-WFP-1 (b) MoS2 (c) nitrogen adsorption–desorption isotherms of MoS2 and (d) hydrodynamic size plot of MoS2 dispersion analyzed by the DLS technique. | ||
Fig. 1d represents the hydrodynamic size plot of solvothermally synthesized MoS2 dispersion analyzed by the DLS technique corresponded to 300 nm. The zeta potential of MoS2 was ca. −20.9 mV, which suggested that the synthesized MoS2 has negatively charged surface (see Fig. S1 in SI).
To further understand the interaction between the substrate (WFP) and the prepared MoS2 ink, the XPS spectra of MoS2-WFP-1 was investigated. The full scan survey spectrum along with deconvoluted Mo and S peaks are provided in Fig. 2a–d. Fig. 2a represents the wide-scan XPS survey spectrum of MoS2-WFP-1 and displays prominent peaks corresponding to molybdenum (Mo), sulfur (S), carbon (C) and oxygen (O). The strong Mo and S signals confirm the presence of MoS2, while the C and O peaks are attributed mainly to the cellulose substrate of the WFP and possible adventitious carbon. The high-resolution Mo 3d spectrum typically in the region between 224 to 237 eV (Fig. 2b), showed major peaks for Mo 3d5/2 and Mo 3d3/2 at 228.78 and 232.00 eV, respectively. These binding energies are characteristic of Mo4+ in the 1T phase of MoS2 (48.7%, calculated based on peak area), indicating that the solvothermal synthesis and screen-printing process preserved the desired oxidation state and structure of molybdenum. The other pair of peaks at 230.04 and 232.91 eV corresponding to the 2H phase of MoS2 (32.6%). The coexistence of 2H and 1T phases (as detected by XPS) is often beneficial, combining stability (2H) with reactivity (1T).37 The peak at higher binding energies (235.63 eV for Mo6+) indicates the presence of MoO3 (7.7%) or other higher-valence states, which are usually observed in the synthesized MoS2 by hydrothermal or solvothermal methods.38–41 The presence of mixed phase MoS2 was further confirmed by Raman analysis (Fig. 3). The other shoulder peak at 226.31 eV corresponding to the S 2s, due to emission from the defect-free regions of MoS2 (11%).
Fig. 2c represents the high-resolution spectrum of S 2p. The two major peaks at 161.83 eV and 163.16 eV corresponding to the characteristic peaks of S2− in MoS2 which come from the majority of sulfur present in the desired sulfide state.42 There are no significant peaks corresponding to oxidized sulfur species such as SO42−, indicating no sulfur oxidation. The S
:
Mo atomic ratio, calculated from XPS data remains close to the ideal value of 2
:
1, further supporting the predominance of MoS2. In Fig. 2a, the peak of C 1s at 284.8 eV, and O 1s at 532.2 eV, are attributed to the cellulose matrix of the WFP and the adsorbed MoS2 species. The deconvoluted C 1s spectra confirms the 4 types of carbons bonds (Fig. 2d), C–C/C–H, C–O, C
O and O–C
O at 284.8, 286.25, 286.93 and 287.9 eV, respectively.43 The significant C–O and O–C
O groups on the cellulose WFP surface provide abundant sites for hydrogen bonding44 with sulfur atoms or oxygen-containing groups on MoS2. The polar nature of the oxygenated carbon species increases the surface energy of the cellulose,45 promoting better wetting and adhesion of the MoS2 ink during screen printing. The preservation of the chemical structure of cellulose, as evidenced by C–C/C–H peak, ensures that the filter retains its fibrous, porous morphology, which physically entraps MoS2 nanoflakes. The preservation of fibrous morphology was further confirmed by FESEM images.
The Raman spectrum shown in Fig. 3 confirms the successful formation of mixed-phase MoS2 containing both 1T and 2H phase. The co-existence of these phases is evidenced by the appearance of characteristic vibrational modes corresponding to both crystal structures. The two prominent peaks at approximately 378 and 402 cm−1 correspond to the characteristic Raman-active modes of 2H–MoS2. The peak at 378 cm−1 is assigned to the in-plane E12g mode, arising from the opposite in-plane vibrations of Mo and S atoms, while the peak at 402 cm−1 corresponds to the out-of-plane A1g mode, mainly associated with sulphur atom vibrations perpendicular to the MoS2 layers. In addition to these peaks, the characteristic of 1T phase peaks are observed at low frequency range referring to J1, J2 and J3 modes.46 These J peaks are presumed to originate from symmetry lowering and structural rearrangement from the stable 2H phase to the metastable metallic 1T phase.
The FESEM micrographs of WFP and MoS2-WFP-1 are provided in Fig. 4a and b. The fine fibrous and porous morphology for pristine WFP is observed in Fig. 4a. The cellulose fibers, typically measuring micrometers in diameter, are randomly interwoven, creating a three-dimensional matrix with interconnected pores. This structure is ideal for filtration, allowing for high water permeability and providing a large surface area for subsequent functionalization. With the screen-printing of prepared MoS2 ink on WFP (Fig. 4b and b(1)), the cellulose fibers were coated with a continuous, conformal layer of MoS2 nanoflakes. The coating appears as a textured sheath enveloping the fibers, indicating strong adhesion and effective coverage. At higher magnification, the MoS2 layer is composed of overlapping, plate-like nanoflakes of nanometer dimensions.
The surface of the coated fibers is significantly rougher than that of the bare cellulose, due to stacking of MoS2 nanosheets. The increased roughness of WFP after screen printing of MoS2 is supplemented by AFM analysis and the images are provided in Fig. 5. The pristine WFP presented smoother surface compared to the MoS2 screen printed one. The appearance of pronounced ridges, valleys, and aggregated domains for the MoS2 printed membrane clearly indicated the increased roughness. The average roughness of WFP and MoS2-WFP-1, measured at 5 different positions is found to be 19.53 and 30.25 nm, respectively, which clearly quantifies the increased surface roughness. This roughness increases the effective surface area, which is beneficial for adsorption and catalytic applications.
Along with the morphology, EDX mapping was performed to confirm the presence and atomic ratio of Mo and S in MoS2-WFP-1. The results are displayed in Fig. 6. The atomic percentage for Mo and S are 33.57 and 66.43%, respectively, which is expected for MoS2. The mapping showed the distribution of Mo and S throughout the WFP surface indicating the uniformity of the surface.
![]() | ||
| Fig. 6 (a) Elemental composition; (b) respective FESEM image; (c) and (d) elemental mapping for Mo and S, respectively for MoS2-WFP-1. | ||
Following the examination of surface morphology, the study was extended to analyze the mechanical and thermal stabilities of the prepared membranes. The thermo-gravimetric analysis performed for WFP and MoS2-WFP-1 is given in Fig. 7a, and stress vs. strain graphs predicting mechanical strengths for all the membranes are provided in Fig. 7b. For the WFP membrane, a sharp weight loss begins around 310 °C, corresponding to the rapid decomposition of the cellulose. Complete degradation occurs before 400 °C, with minimal residual mass, which indicates thermal stability. For the MoS2 printed filter, the initial thermal decomposition started at a similar temperature as that of WFP, but progressed more gradually than the uncoated paper. The residual mass remaining even after 800 °C (around 12%) is attributed to a thermally stable MoS2 phase.
![]() | ||
| Fig. 7 (a) TGA curves for WFP and MoS2-WFP-1; (b) stress vs. strain curves for all fabricated membranes along with WFP. | ||
The presence of MoS2 on WFP, delayed the onset of degradation and reduced the rate of mass loss. The stress–strain behavior of the fabricated membranes under tensile loading were investigated. The WFP membrane exhibited a higher initial stress response, but broke at a relatively low strain (0.67%). The curve showed a sharp drop after the peak, indicating the brittle fracture, which is typical for unsupplemented cellulose networks. With increased number of prints of MoS2 on the WFP, the strain at break increased to 0.84, 1.13 and 1.18%, with increasing prints of MoS2. Along with increased stress at peak, it is also observed that, the ductile and tough nature of the fabricated membranes also enhanced. The MoS2 filling the cellulose matrix could bridge the gaps between the cellulose fibers, which could distribute the stress more evenly and prevent premature fiber fracture and hence the increased ductile nature. It is also noted that, with an increasing number of prints (layers), the strain-at-break increases, confirming that the nanocoating directly reinforces the fibrous matrix. The enhanced thermal as well as mechanical stability of WFP membranes with MoS2 coating is advantageous for the regeneration of the membrane as well as usage of membranes for long-term water treatment, when compared to the bare WFP membrane.
![]() | ||
| Fig. 8 (a) Pure water flux; (b) water uptake for WFP, MoS2-WFP-1, MoS2-WFP-2 and MoS2-WFP-3 membranes. | ||
Reported pure water fluxes for MoS2-based membranes vary widely depending on fabrication method, thickness, and support material. For example, MoS2/GO composite membranes have shown fluxes from 8.8 to 48.3 L m−2 h−1, while pure MoS2 nanosheet membranes can achieve 30–250 L m−2 h−1 bar−1 under pressure-driven conditions.47–49 The values observed here for screen-printed MoS2-WFP membranes are consistent with these reports, especially considering the absence of external pressure in gravity-driven filtration.
Along with PWF, water uptake studies were also performed to understand the water absorption ability of the fabricated membranes. The results are provided in Fig. 8b. The WFP membrane presented a WU of 49.6% (mean) and for MoS2 coated membranes, the WU increased to 53.5 to 55.5%. Despite increased hydrophobicity, the WU remained almost same. This indicates that, MoS2 layers, while making the surface hydrophobic, did not fully prevent bulk water adsorption. This could be due to the retention of hydrophilic sites by cellulose and the access provided by the porous structure. The measured average contact angles for WFP, MoS2-WFP-1, MoS2-WFP-2 and MoS2-WFP-3 are of 25.9, 104.7, 108.6 and 118.1°, respectively (the photographs are presented in Fig. 6b). When compared to WFP membranes, MoS2-coated membranes showed a dramatic rise in CA to above 100°, thus demonstrating increased hydrophobicity, as MoS2 nanoflakes were layered. With increased print layers, the CA further increased, but the changes were insignificant. Despite enhanced surface hydrophobicity with respect to increased number of prints or coats, the bulk water uptake remained high. This is due to water absorption driven by internal hydrophilic cellulose, as well as the surface. Moderate porosity was preserved within the cellulose matrix even after 3 coats of MoS2, hence, obtaining the PWF and water uptake.
Fig. 9c, 10c and 11c present the permeate flux at different pH and demonstrate a generally stable flux, with only minor fluctuations. A slight flux decrease at extreme pH conditions suggests minor swelling, or interactions between the membranes and solution components, but overall, the flux was maintained. This indicates the good chemical robustness of the membranes. The removal efficiency of the MoS2-WFP-1 membrane towards CR, MB and Cr(VI) at different pH conditions is provided in Fig. 9d, 10d and 11d, respectively. For a better understanding of the mechanism involved, the zeta potentials of all three considered contaminants at varied pH was measured and the results are provided in SI as Table S1 and Fig. S2 to S10.
CR, being an anionic dye, was removed by ∼90.3% at acidic pH and the removal then dropped to ∼63% in basic pH (Fig. 9d). At acidic pH, the negative MoS2 surface (zeta potential −20.9 mV) is protonated and is therefore expected to favor electrostatic attraction toward the anionic CR. The zeta potential of CR becomes increasingly negative with increasing pH (−40.8 mV at pH 4 to −65.5 mV at pH 9), removal efficiency decreased correspondingly. Since both the membrane and CR possess negative surface charges, stronger electrostatic repulsion at higher pH reduces rejection efficiency. The comparatively higher removal at pH 4 may be attributed to weaker electrostatic repulsion.
In the case of MB, the dye exhibits a positive zeta potential at pH 4 (+16.0 mV), resulting in strong electrostatic attraction toward the negatively charged membrane and enhanced removal behaviour. As the pH increases, the zeta potential becomes slightly negative (−7.37 to −9.41 mV), reducing attractive interactions. Nevertheless, moderate rejection is still observed, likely due to adsorption and steric hindrance effects.
For Cr species, the zeta potential remains negative across the investigated pH range. The maximum removal of about 72% (Fig. 11d) was achieved at a lower pH for Cr(VI), owing to the anionic forms of Cr(VI), such as HCrO4− and Cr2O72−. At low pH, the protonated, positively charged MoS2 surface strongly attracts these anions. Reductive adsorption (and possible partial reduction to Cr(III)) is also favored under acidic conditions. Overall, the work validates MoS2 ink printing as a green, low-cost route to fabricate high-strength, reusable nanocomposite paper membranes, establishing a foundation for future scaling, and optimization towards heavy metal and organic contaminant remediation systems.
![]() | ||
| Fig. 12 ATR-IR spectra of WFP, MoS2-WFP-1 (before use) and MoS2-WFP-1 (after acid treatment for 16 h). | ||
After MoS2 coating, noticeable changes in spectral intensity and band profile are observed for MoS2-WFP-1, confirming successful deposition of the MoS2 layer over the cellulose substrate. The reduction in intensity of cellulose-related bands suggests partial surface coverage of the WFP fibers by MoS2 sheets. Slight broadening and suppression of the hydroxyl and C–O vibration bands further indicate interfacial interactions between the MoS2 coating and cellulose network.
The ATR-IR spectrum of the membrane after immersion in dilute acid and subsequent washing remains highly similar to that of the membrane before use. Minor intensity variations observed after washing may arise from partial removal of loosely attached particles. However, the absence of significant spectral alterations confirms that the membrane structure remains largely intact and the coated layer maintains good adhesion to the WFP substrate even after chemical exposure and washing treatment.
Supplementary information (SI): the zeta potential plots of MoS2 and all three contaminants under different pH conditions. See DOI: https://doi.org/10.1039/d6ra01189f.