Open Access Article
Hae In
Lee†
a,
Myung Won
Seo†
b,
Dong Hyun
Kim
c,
Hyuk
Choi
d,
Ju Hyeok
Lee
d,
Mi
Yoo
d,
Min-Jae
Kim
c,
Yong-Sik
Ok
e,
Siddheshwar Dadarao
Raut
f,
Dong Hyun
Lee
f,
Hyun You
Kim
*d,
Kyubock
Lee
*c and
Won-Chul
Cho
*f
aSchool of Energy and Chemical Engineering, Ulsan National Institute of Science and Technology, Ulsan 44919, Republic of Korea
bSchool of Environmental Engineering, University of Seoul, Seoul 02504, Republic of Korea
cGraduate School of Energy Science & Technology, Chungnam National University, Daejeon 34134, Republic of Korea. E-mail: kyubock.lee@cnu.ac.kr
dDepartment of Materials Science and Engineering, Chungnam National University, Daejeon 34134, Republic of Korea. E-mail: kimhy@cnu.ac.kr
eKorea Biochar Research Center & Division of Environmental Science and Ecological Engineering, Korea University, Seoul 02841, Republic of Korea
fDepartment of Future Energy Convergence, Seoul National University of Science & Technology, Seoul 01811, Republic of Korea. E-mail: wonchul.cho@seoultech.ac.kr
First published on 8th October 2025
Silicon carbide (SiC) is a critical material across structural, electronic, and catalytic applications; however, its conventional synthesis via the Acheson process is highly energy-intensive, operating at 2200–2400 °C with low carbon efficiency. Herein, we report a novel, solvent-free mechanochemical synthesis of mesoporous SiC using CO2 as a sustainable carbon feedstock and SiO2/Mg as earth-abundant precursors. Through a two-step ball-milling process, SiO2 is first reduced by Mg to form Mg2Si, which then spontaneously reacts with CO2 to form SiC and MgO, achieving a high CO2 conversion efficiency of 84% at only 10% of the energy cost of conventional methods. Density functional theory (DFT) calculations confirm the thermodynamic feasibility of CO2 activation on Mg2Si. The produced mesoporous SiC exhibited excellent durability and served as a highly stable support for Ni catalysts in dry reforming of methane (CH4 + CO2 → H2 + CO), maintaining performance over 100 hours with minimal coke formation. This work introduces a green, scalable route for synthesizing high-value SiC, integrating CO2 utilization and catalyst development under the principles of green chemistry.
Here, we instead formulate a concrete economic value chain covering efficient CO2 conversion to value-added products. We focus on silicon carbide, SiC, a vital material in structural, electronic, and energy applications, to maximize the economic impact.9 Commercial SiC powders are typically produced by the energy-consuming Acheson process (SiO2(s) + 3C(s) → SiC(s) + 2CO(g)).10 The Acheson process lasts for several hours (up to 30 h) and involves a long, direct carbothermic reaction of quartz sand and petroleum with low commercial yields of ∼19% at extremely high temperatures (∼2200–2400 °C).11 A general Acheson process consumes 7300–7600 kW h of energy to produce a metric ton of SiC, equivalent to the total energy stored in approximately 100 fully charged electric vehicles.12 Moreover, because the produced α-SiC particles are large and highly crystalline, mechanical milling and subsequent conversion into relatively novel β-SiC powders through carbothermic reduction should be performed.13 The quality of the produced SiC can be improved using higher-grade resources such as a stoichiometric mixture of metallic Si particles of d < 20 μm and C powders for carbothermic reduction14 or a mixture of activated C and Si (or silica) for microwave processing.15 However, these approaches are also time-consuming and cost-ineffective.
Inspired by the mechanochemical conversion method,16–19 we designed a straightforward and cost-effective method of synthesizing high-quality SiC using CO2 as a carbon resource. In this approach, a mixture of nano-SiO2 particles (nsp) and Mg is initially converted into Mg2Si, a key intermediate, via ball-milling. The strong interaction between Mg2Si and CO2 activates the subsequent transformation of Mg2Si into mesoporous SiC. The advanced multifunctional SiC synthesis reported herein provides an intelligent route for producing high-quality SiC with a high carbon conversion efficiency of 84%. Our mechanochemical synthesis method provides a means of directly utilizing CO2 in value-added metal carbides. In addition, the applicability and quality of our mechanochemically produced mesoporous SiC were confirmed by the excellent efficiency and consistency of the Ni/SiC catalysts toward dry reforming of methane (DRM).
Fig. 1a provides a schematic of a two-step, ball-milling-based sequential mechanochemical SiC synthesis process. During the reaction, Mg reduces SiO2-nsp and produces Mg2Si, a crucial substance in the overall process. The second subsequent mechanochemical reaction converts a mixture of Mg2Si and CO2 into SiC and MgO. The high-resolution transmission electron microscopy (HR-TEM) images reveal the morphology of the produced SiC-nsp particles (Fig. 1b–d). The synthesized SiC-nsp particles exhibit mesoporous textures composed of single-crystalline primary SiC nanoparticles with a typical [111] interlayer spacing of β-SiC (0.252 nm) (Fig. 1b–d and SI Fig. 1 and 2).
The density functional theory (DFT)-calculated energetics of CO2 binding and dissociation on the surface of Mg2Si nanoparticles confirm that Mg2Si binds and activates CO2 (Fig. 1e). Up to 10 CO2 molecules are exothermically bound to a single Mg2Si nanoparticle (Ebind = −1.69 eV per CO2), and the subsequent dissociation steps are thermodynamically driven with ΔE = −1.18 eV per CO2, which originates from the atomic-scale formation of SiC and MgO units within the matrix of a Mg2Si nanoparticle (Fig. 1e). Additional calculations performed with three representative Mg2Si surfaces reveal that the binding and dissociation of CO2 on Mg2Si is energetically feasible (SI Fig. 3).
The reaction pressure profile presented as a function of the reaction time shows that the conversion occurs fairly rapidly after 150 s of incubation time (Fig. 2a). The X-ray diffraction (XRD) spectra show that Mg2Si and MgO are the primary products of the first ball-milling step (Fig. 2b). The pressure–reaction time profile presented in Fig. 2c demonstrates that the second conversion is completed within 40 s, generating a mixture of SiC and MgO from Mg2Si and CO2. Note that CO2 is the sole carbon resource for the carbonization of Mg2Si to SiC. Remarkably, the reaction proceeds adiabatically without any energy supply from the outside. The final product, SiC-nsp, was obtained after sequential acid-base leaching. The XRD pattern of the finally produced SiC powder confirms the primary peaks of β-SiC. No amorphous carbon layer (ACL) was found on the surface of SiC-nsp (SI Fig. 2).
The N2 adsorption–desorption isotherms of nsp and SiC-nsp are shown as type-II profiles (Fig. 2e). The overall trend of the hysteresis loops of nsp and SiC-nsp displays a typical type-H3 profile, which represents non-rigid aggregates of particles, consistent with the electron microscope observations (SI Fig. 1), while the H3 hysteresis also suggests additional interparticle voids that can extend toward the macropore regime. The Barrett–Joyner–Halenda (BJH) pore-size distributions reveal that the mesopore structures of nsp and SiC-nsp are similar to each other (Fig. 2f). The decreased surface area and pore volume of SiC-nsp (140 m2 g−1 and 0.30 cm3 g−1, respectively) compared to those of nsp (195 m2 g−1 and 0.41 cm3 g−1, respectively) are presumably due to the slight particle aggregation that occurred during ball milling (SI Tables 1 and 2). The similar morphological features in the N2 adsorption–desorption isotherms and the BJH pore diameter distribution profiles of nsp and SiC-nsp show that the initial microstructure of the SiO2 resource (nsp) is conserved in the final mechanochemically produced SiC (SiC-nsp). Our mechanochemical conversion method provides a novel route toward intentional control of the morphology of SiC, based on efficient conversion of SiO2 through the solid–gas reaction, which is not available in the commercial Acheson process by the solid–solid reaction.
Value-added porous sub-micron SiC powders (approximately USD 300 per kg) could be produced by our mechanochemical synthesis using low-cost and readily available commercial materials such as nano-SiO2 (USD 2 per kg), Mg (USD 10 per kg), and CO2 (USD 0.06 per kg) via simple milling processes. An almost stoichiometric amount of CO2 was utilized to produce SiC; 3.4 g of SiC was obtained from 4.4 g of CO2, corresponding to a yield of 84% for CO2–SiC conversion.
To explore the versatility of our mechanochemical SiC synthesis method, we repeated the two-step ball-milling process using a naturally porous rice husk silica (rha) as a biomass-based alternative owing to its large-scale global availability (∼70 million tons were produced in 2012). The XRD patterns, scanning electron microscopy (SEM) images, and TEM images concurrently confirm that porous SiC (SiC-rha) is produced using rha as the SiO2 source (Fig. 3a and SI Fig. 4). These findings suggest that our mechanochemical SiC synthesis method is highly versatile and adaptable to various situations, regardless of the quality and type of the SiO2 source. We further applied the conventionally used powder-activated carbon (AC) instead of CO2 as a carbon source in the ball-milling cycle with the nsp. The SiC synthesized with AC (SiC-nsp-ac) exhibits a higher Si peak intensity in the XRD spectra (SI Fig. 5), suggesting a lower conversion efficiency of solid-phase AC compared to gaseous CO2. In addition, the unreacted AC during the milling process generates an ACL on the surface of SiC-nsp-ac (Fig. 3c). The thermogravimetric analysis (TGA) curve shows that the SiC-nsp-ac undergoes noticeable weight loss between 460 °C and 550 °C, which can be attributed to the oxidation of the residual carbon (Fig. 3d). Our results show that reactive Mg2Si intermediate enables gaseous CO2 to interact vigorously with solid substances despite its general chemical inertness.
Chemical durability is among the key strengths of SiC in industrial applications.20 The surface area and elemental composition of the mechanochemically produced SiC presented herein do not show any considerable changes after exposure to harsh acidic and basic conditions for three weeks (SI Table 3). Based on the inherent physicochemical robustness of SiC, various promising catalytic reactions have been performed using β-SiC as a catalyst or catalyst support.21–25 One of the key characteristics of a catalyst or catalyst support is a high surface area that has hardly been achieved for β-SiC produced through the high-temperature Acheson process.11 We applied the mechanochemically produced mesoporous SiC-nsp as a support for Ni-based DRM catalysts (Ni/SiC-nsp, specific surface area = 79 m2 g; SI Table 4) that convert the two most significant greenhouse gases (CH4 and CO2) into industrially valuable syngas (H2 and CO).26–28
Therefore, we suggest a two-step sequential CO2 utilization process via mechanochemical SiC synthesis followed by DRM catalysis by Ni/SiC-nsp, as shown in Fig. 4a. The TEM and energy-dispersive X-ray spectroscopy mapping images of the catalysts after Ni and Mg impregnation as the active sites and promotors reveal homogeneously dispersed Ni nanoparticles with an average size of 19.7 nm on the SiC support (Fig. 4b). The homogeneous dispersion and fine particle size of the active sites originate from the mesoporosity of SiC. The DRM reaction test results in Fig. 4c show that the Ni/SiC-nsp catalyst consistently catalyzes the DRM reaction with the CH4 and CO2 conversions close to thermodynamic equilibrium for 100 h without significant reduction.
![]() | ||
Fig. 4 Mesoporous Ni/SiC catalysts in the DRM reaction. (a) Schematic diagram of a two-step sequential CO2 utilization process via mechanochemical SiC synthesis followed by DRM catalyzed by Ni/SiC-nsp, (b) TEM images with HAADF and EDS mapping of Ni/SiC-nsp catalyst, (c) CO2 and CH4 conversion during a 100 h DRM reaction at 800 °C and a 10 000 mL g−1 h−1, of WHSV where the dashed lines indicate each conversion at thermodynamic equilibrium, (d) comparison of the stability and coke resistance of Ni/SiC-nsp with those of previously reported DRM catalysts.25–36 | ||
Remarkably, the resistance against coke deposition of the catalyst, the most significant challenge hindering the commercialization of DRM catalysts, evaluated by TGA after 100 h of reaction revealed only 1.71 wt% coke deposition on the Ni/SiC-nsp, which corresponds to 0.174 mgcoke gcat−1 h−1 (Fig. 4d). These results demonstrate the superior performance of SiC-nsp as a catalyst support for high-temperature reactions. The stability and coke resistance of Ni/SiC-nsp (as indicated by the red star symbol) is compatible with the recently reported high-performance DRM catalysts (as denoted by the black rectangular symbols), prevailing those of the previously reported SiC-based Ni catalyst (red rectangular symbol).29–40 For large-scale and high-temperature catalysis, overcoming cold or hot spots on the catalyst bed and enduring thermal shocks during operation are of great importance for the performance and stability of the catalytic reaction. Considering that the most fascinating characteristics of SiC as the catalyst or catalyst support are its high thermal conductivity and stability,41,42 our mesoporous SiC is highly applicable in various catalytic systems.
![]() | (1) |
![]() | (2) |
![]() | (3) |
The reaction between the gas (CO2) and solid particles occurs when the energy reaches a certain level inside the vial. The reaction was mainly induced by the collision energy rather than the thermal energy at high temperatures to overcome the activation barrier, a process referred to as mechanochemistry.1 Acid and base leaching was respectively performed using 10 wt% HCl and 1 M NaOH solution for the resulting SiC–MgO composite to remove MgO and other impurities from the balls and vials, yielding the final porous SiC. Nanosilica particles (∼20 nm) and rice-husk-derived SiO2 were used as the Si sources, and AC (SHIRASAGI) was employed as a C source and control. AC was placed in a vial in a glove box system maintained under an Ar atmosphere.
The CO2 to SiC yield is defined and calculated as follows:
![]() | (4) |
:
1
:
1 ratio flowing at a weight hourly space velocity (WHSV) of 10
000 mL g−1 h−1. The reactions were conducted at 800 °C for 100 h. The outlet gas was analyzed every 22 min by an online gas chromatography system equipped with a thermal conductivity detector. The conversions are as follows:![]() | (5) |
![]() | (6) |
An octahedral Mg158Si79 particle located inside a 40 × 40 × 40 cell was used to study the energetics of CO2 binding and the formation of SiO2 and SiC. The average binding energy (Ebind) of CO2 on Mg2Si and the subsequent dissociation energy (ΔE) were estimated by averaging Ebind and ΔE of a total of 10 CO2 molecules. To explore the inherent CO2 binding and dissociation capacity of Mg2Si further, Ebind and ΔE were calculated on pristine Mg2Si surfaces, i.e., Mg2Si (100), Mg2Si (110), and Mg2Si (111). Next, (3 × 3 × 2), (3 × 4 × 3), and (4 × 4 × 2) supercells were used to model the Mg2Si (100), Mg2Si (110), and Mg2Si (111) surfaces, respectively. The bottom-most layer of the slab model was fixed during the geometry optimization. A 15 Å thick vacuum layer was introduced to prevent interactions between the periodic slabs.
Footnote |
| † These authors contributed equally to this study. |
| This journal is © The Royal Society of Chemistry 2026 |