Molten salt synthesis of Eu2+-doped Sr5(PO4)3Cl in air atmosphere: europium self-reduction and optical properties

Simona Bendziute a, Jonas Stadulis a, Guna Doke ab, Guna Krieke ab, Andris Antuzevics b, Vladimir Pankratov b, Inga Grigoraviciute a, Arturas Katelnikovas a and Aleksej Zarkov *a
aInstitute of Chemistry, Vilnius University, Naugarduko 24, LT-03225 Vilnius, Lithuania. E-mail: aleksej.zarkov@chf.vu.lt
bInstitute of Solid State Physics, University of Latvia, Kengaraga 8, LV-1063 Riga, Latvia

Received 3rd November 2025 , Accepted 19th January 2026

First published on 26th January 2026


Abstract

In the present work, a series of Eu2+-doped Sr5(PO4)3Cl powders with varying Eu content was synthesized by the molten salt method in an air atmosphere. The self-reduction of Eu3+ to Eu2+ occurred during the phase transformation of starting Sr3(PO4)2:Eu to Sr5(PO4)3Cl:Eu in molten SrCl2. The synthesis conditions were optimized in terms of reaction temperature, time, and precursor-to-flux ratio. The optical properties of the obtained materials were investigated through photoluminescence, thermally stimulated luminescence, and persistent luminescence decay measurements. Regardless of the Eu concentration, the resulting powders possessed a dominating Eu2+-related broadband emission with a maximum at 445 nm; however, significantly weaker emission in the red region was also detected, suggesting incomplete reduction of Eu3+ to Eu2+. Minor emission tunability was achieved by varying the excitation wavelength, which allows for the elimination of Eu3+ emission. The analysis of trap properties indicated the presence of two types of traps. Although all obtained Ea values were deep, a weak persistent luminescence signal of Eu2+ can be detected for several hours after X-ray irradiation.


1. Introduction

The Eu2+ ion is one of the most frequently used activators in luminescent materials due to its exceptional optical properties, which include broad excitation and absorption bands, as well as intense broadband emission, originating from the dipole and spin allowed 4f65d1 → 4f7 transitions.1,2 Moreover, the local coordination environment has a significant effect on the emission of Eu2+ ions, resulting in the matrix-dependent luminescence covering a broad spectral range from blue to infrared.3 Due to these properties, Eu2+-doped materials have been widely investigated for applications in white light-emitting diodes, scintillators, long afterglow phosphors, etc.4–6

Most frequently, Eu2+-activated phosphors are synthesized in a reducing atmosphere, which is caused by the need to convert Eu ions from trivalent to divalent oxidation state. However, some specific matrices allow the reduction of Eu3+ to Eu2+ in the air atmosphere, which is defined as Eu self-reduction.7 The self-reduction phenomenon has several requirements for the matrix, which usually include: (I) the absence of oxidizing ions in the host compound; (II) the Eu3+ dopant replaces a divalent cation in the host; (III) the substituted cation has a similar radius to that of Eu2+; and (IV) the host material has a crystal structure, based on tetrahedral anion groups ([SiO4]4−, [PO4]3− or [AlO4]5−, etc.).8 Obviously, the self-reduction strategy offers multiple advantages over the use of reducing environment in terms of lower price, safer and easier handling; however, the choice of suitable hosts is limited. Although the self-reduction of Eu3+ is most frequently incomplete, resulting in mixed-valence materials, in some cases, this fact can be considered as an advantage, e.g., realizing a dual-emitting material with tunable luminescence.9 Tuning the emission by varying excitation wavelength, temperature, or pressure can result in selective or simultaneous emission of Eu2+/Eu3+ species. Such materials can be used for anti-counterfeiting or luminescent thermometry and manometry.10–12

Sr5(PO4)3Cl is a perfect candidate for realizing Eu3+ to Eu2+ self-reduction since this host meets all the above-mentioned matrix requirements. Moreover, the ionic radii of Sr2+ and Eu2+ (1.26 Å and 1.25 Å for VIII-fold coordination, as expected in Sr5(PO4)3Cl, respectively) are almost identical.13 Sr5(PO4)3Cl belongs to the family of apatite-structure materials, known for their structural flexibility and ability to adopt both isovalent and aliovalent ions.14,15 For this reason, many alkaline earth apatite-type phosphors were previously developed by doping the matrix with various rare-earth ions.9,16–19 The synthesis of Eu2+-doped Sr5(PO4)3Cl is also described in the literature; however, the reported synthesis conditions and resulting luminescent properties vary significantly. Although most studies combine the conventional solid-state reaction method with a reducing H2 or CO atmosphere,20–25 there are few reports on the synthesis of mixed-valence Eu-doped Sr5(PO4)3Cl in air.26–28 For instance, Deng et al. reported Eu2+ emission in Sr5(PO4)3FxCl1−x solid solutions synthesized in air; however, the spectral range corresponding to Eu3+ emission was not shown.27 Mixed-valence Sr5(PO4)3Cl:Eu was previously synthesized by Chen et al. by the solid-state reaction method in air.28 The observed Eu2+/Eu3+ emission was concentration-dependent, allowing for the achievement of tunable luminescence by varying Eu content. A wet-chemical approach to the synthesis of Eu2+-doped Sr5(PO4)3Cl was demonstrated in a very few works. Song et al. used hydrazine as a reducing agent under hydrothermal conditions.29 The ratio of Eu2+ and Eu3+ emission was dependent on the hydrazine concentration, chemical reaction duration, and excitation wavelength. Zou et al. employed a solvothermal approach using various organic additives, which makes the reason for Eu3+ reduction unclear.30

In the present work, we report the synthesis of Eu2+-doped Sr5(PO4)3Cl by the molten salt method in an air atmosphere. The self-reduction of Eu3+ to Eu2+ occurred during the phase transformation of Sr3(PO4)2:Eu precursor to Sr5(PO4)3Cl:Eu in molten SrCl2. The luminescent properties of the resulting materials were studied in terms of steady-state and kinetic luminescence, thermally stimulated luminescence, and persistent luminescence decay measurements.

2. Experimental

2.1. Synthesis

The synthesis of Sr5(PO4)3Cl:Eu powders was performed by a two-step procedure. In the first step, a series of Sr3(PO4)2 powders with different amounts of Eu3+ was synthesized by the co-precipitation method, followed by high-temperature annealing. The Eu doping level (0.1, 0.25, 0.5, 1.0, and 2.0 mol%) was calculated with respect to Sr2+ ions. Sr(NO3)2 (≥99%, Roth), (NH4)2HPO4 (≥98%, Roth), and Eu(NO3)3·6H2O (99.9%, Acros Organics) were used as starting materials. For the synthesis, the appropriate amounts of Sr(NO3)2 and Eu(NO3)3·6H2O were dissolved in 50 mL of deionized water to obtain a solution with a total concentration of metal ions of 0.6 M. In parallel, (NH4)2HPO4 was dissolved in 50 mL of deionized water in a separate beaker to obtain a 0.4 M solution. The pH value of the phosphate solution was adjusted to 10 with ammonia solution (NH4OH, 25%, Roth). The solution of metal nitrates was rapidly added to the (NH4)2HPO4 solution, resulting in the formation of white precipitates. The obtained precipitates were aged for 10 min, filtered, washed with deionized water to remove residual counterions, and dried in an oven at 80 °C overnight. The resulting powders were ground in an agate mortar and annealed in a furnace in air at 1100 °C for 5 h at a heating rate of 5 °C min−1.

In the second step, Sr3(PO4)2:Eu was converted to Sr5(PO4)3Cl:Eu by the molten salt method. For the synthesis, 1 g of Sr3(PO4)2:Eu was thoroughly mixed with SrCl2 (≥95%, Thermo Scientific) at a mass ratio of 1[thin space (1/6-em)]:[thin space (1/6-em)]2, respectively. The obtained mixture was transferred into the corundum crucible, covered with a lid, heated in air to 1000 °C at a rate of 5 °C min−1, and annealed at this temperature for 1 h. After the annealing procedure, the furnace was cooled down naturally. The melts were washed with hot deionized water to dissolve residual SrCl2. Finally, the products were dried in an oven at 80 °C and ground in a mortar. The Sr5(PO4)3Cl:Eu samples in the text are denoted according to the nominal Eu content in Sr3(PO4)2:Eu precursors.

2.2. Characterization

Powder X-ray diffraction (XRD) data of the synthesized powders were obtained using a Rigaku MiniFlex II diffractometer (Cu-Kα, λ = 1.5419 Å) working in the Bragg–Brentano (θ/2θ) geometry. The data were collected within the 10–60° 2θ angle range with a 5° min−1 scan speed.

Fourier transform infrared (FTIR) spectra were taken in the 4000–400 cm−1 range using a Bruker ALPHA-FTIR spectrometer.

Raman spectra were recorded by a combined Raman and scanning near-field optical microscope WiTec Alpha 300 R equipped with a 532 nm excitation laser source.

The morphology of the synthesized powders and elemental distribution were studied by scanning electron microscopy (SEM) with coupled energy-dispersive X-ray spectroscopy (EDX) using a FlexSEM 1000 II microscope.

The Eu content in the synthesized products was quantified by inductively coupled plasma optical emission spectrometry (ICP-OES) using a PerkinElmer Optima 7000DV spectrometer. The samples prior to analysis were dissolved in 5% nitric acid (HNO3, Rotipuran® Supra 69%, Roth).

The photoluminescence excitation (PLE) and photoluminescence emission (PL) spectra were measured using the Edinburgh Instruments FLS980 spectrometer equipped with double excitation and emission monochromators, a 450 W Xe arc lamp, a cooled (−20 °C) single-photon counting photomultiplier (Hamamatsu R928P), and mirror optics for the powder samples. The PL spectra were corrected using a correction file obtained from a tungsten incandescent lamp certified by NPL (National Physics Laboratory, UK). The excitation spectra were corrected by a reference detector. PL decay curves were measured using the same Edinburgh Instruments FLS980 spectrometer.

For PL decay measurements, a picosecond pulsed diode laser from Edinburgh Instruments (EPL-405) was used as an excitation source (λex = 405 nm).

Quantum yields (QY) were determined using a Teflon-coated integrating sphere and a barium sulfate (BaSO4 for white standard DIN 5033, Merck) as a white standard.31

Thermally stimulated luminescence (TSL) glow curves and spectra, along with persistent luminescence decay measurements, were conducted using the Lexsyg research TSL/OSL reader (Freiberg Instruments GmbH), equipped with a photomultiplier tube R13456 from Hamamatsu and an Andor SR-303i-B spectrometer paired with a DV420A-BU2 CCD camera. For irradiation sources, a VF-50 J/S X-ray tube (40 kV, 0.5 mA, tungsten anode) or a Q-switched short-pulsed UV laser DTL-389QT (263 nm) from the Laser-Compact Group was employed. The system operated with a linear heating rate of 1 °C s−1. Isothermal afterglow decay was measured at 25 °C. To eliminate any effects from previously stored energy, the samples were preheated to 300 °C prior to each measurement.

Room-temperature EPR spectra were measured using a Bruker ELEXSYS-II E500 CW-EPR spectrometer operating at X- (9.834 GHz) and Q- (34.01 GHz) microwave frequency bands and 1 mW microwave power. The magnetic field modulation amplitude was 0.1 mT with a 100 kHz modulation frequency. An X-ray tube operated at 45 kV and 10 mA for 30 min was used to investigate the radiation-induced radicals in the samples. Afterwards, the irradiated samples were isochronally annealed in an air atmosphere, maintaining each temperature step for 10 min, using a custom-built furnace. EPR spectra simulations were performed using EasySpin software.32

3. Results and discussion

The XRD pattern of Sr3(PO4)2 precursor doped with 1 mol% of Eu is shown in Fig. S1 as a representative. As seen, the diffraction peaks match very well with the standard XRD data of rhombohedral Sr3(PO4)2. The PL spectra of Eu-doped Sr3(PO4)2 powders are shown in Fig. S2. Evidently, under a 270 nm excitation, the spectra are dominated by sharp emission lines ranging from orange to the NIR region and associated 4f–4f transitions in Eu3+ ions, specifically 5D07F0–6.33 Only insignificant emission related to Eu2+ was observed, indicating that Eu ions in the precursor are primarily found in a trivalent state, and a low degree of Eu reduction was achieved during the synthesis of Sr3(PO4)2. This observation agrees well with a previous study by Szyszka et al., who reported a weak Eu self-reduction in sol–gel derived Sr3(PO4)2, resulting in a co-existence of mixed-valence Eu ions.34

The synthesis of Sr5(PO4)3Cl:Eu2+ was optimized, aiming to maximize the level of Eu self-reduction and obtain materials with the lowest Eu3+ contribution to the PL spectra. The synthesis conditions were optimized in terms of reaction temperature, time, and precursor-to-flux ratio using a Sr3(PO4)2 precursor doped with 0.1 mol% of Eu. The XRD patterns, normalized PL and PLE spectra of Sr5(PO4)3Cl:Eu powders synthesized at temperatures from 900 to 1100 °C are shown in Fig. S3. Single-phase materials were obtained in all cases; however, the sample synthesized at 900 °C demonstrated the most intense Eu3+ emission, while the difference between the other 2 samples was insignificant. The reaction time in the range from 1 to 10 h did not affect the phase purity (Fig. S4a) and the Eu2+/Eu3+ emission ratio; all the PL spectra were virtually the same (Fig. S4b). Finally, the influence of the precursor-to-flux ratio in the range from 1[thin space (1/6-em)]:[thin space (1/6-em)]1 to 1[thin space (1/6-em)]:[thin space (1/6-em)]10 was investigated. It turned out that the precursor-to-flux ratio did not affect the phase purity of the final products, and the single-phase materials were obtained in all cases (Fig. S5a). On the other hand, the intensity of Eu3+ emission increased with an increase in flux content (Fig. S5b). Based on the obtained results, a final series of Sr5(PO4)3Cl:Eu samples with varying Eu content was synthesized.

Fig. 1a shows the XRD patterns of Sr5(PO4)3Cl:Eu2+ powders obtained by the molten salt synthesis. While the main diffraction peaks match very well with the standard XRD data of hexagonal Sr5(PO4)3Cl, with a P63/m space group (#176), an additional peak was observed at ca. 30° for the samples with higher Eu concentrations starting from 0.5 mol%. The intensity of this peak correlated with the amount of Eu in the starting material; an increase in Eu content corresponded to an increase in intensity. This peak cannot be ascribed to potential secondary phases such as Sr3(PO4)2, EuPO4, EuOCl, or Eu4OCl6. The impurity phase was identified as monoclinic Eu2O3 (PDF-5 #00-034-0072), and the peaks at 14.85° and 29.95° correspond to the (−201) and (−402) planes, respectively. The molten salt method is known for its ability to stabilize metastable materials;35 moreover, it was shown that monoclinic Eu2O3 crystals can be grown from NaF flux.36 We also repeated the synthesis several times; however, the results were reproducible in terms of the presence of the extra peak.


image file: d5dt02634b-f1.tif
Fig. 1 XRD patterns (a), FTIR spectra (b), and Raman spectra (c) of Sr5(PO4)3Cl:Eu powders containing different amounts of Eu.

Vibrational spectroscopy was further employed to confirm the crystal structure and verify the purity of the synthesized powders. The FTIR spectra are shown in Fig. 1b in the spectral range from 1400 to 400 cm−1, since there were no absorption bands in the rest of the spectra. The spectra match well with the results presented in the literature;9,29,37 four groups of bands are clearly seen. The absorption bands in the range from ca. 1110 to 958 cm−1 belong to the asymmetric P–O stretching mode (ν3) of the phosphate tetrahedra, while the band centered at 946 cm−1 is ascribed to the symmetric P–O stretching mode (ν1). The two bands in the range from ca. 615 to 500 cm−1 are attributed to the O–P–O bending mode (ν4) of PO4 units, and the band centered at 459 cm−1 is ascribed to the ν2 O–P–O bending mode. FTIR spectroscopy did not demonstrate any significant differences between the samples based on the Eu content; moreover, the presence of any impurity phase was not detected. This suggests that the impurity phase detected by XRD does not belong to phosphate materials. The Raman spectra of the samples are given in Fig. 1c. Four groups of bands can be seen in all spectra, which agrees with the results of FTIR spectroscopy. The signals observed in the ranges of 400–460, 560–620, and 1010–1080 cm−1 are ascribed to the ν2, ν4, and ν3 vibrational modes of the phosphate group, respectively.25 The most intense band centered at 955 cm−1 corresponds to the ν1 vibrational mode.

The representative SEM images of the synthesized samples are shown in Fig. 2a–c. It is seen that the powders consist of polygonal particles with clearly visible facets. The observed morphology is characteristic of apatite-structure materials prepared by the flux method.38,39 The size of the particles varied in the range from approximately 1 to 6 µm. The amount of Eu did not influence the shape and the size of the obtained particles. Fig. 2d–i demonstrate the EDX mapping of the Sr5(PO4)3Cl:0.25%Eu sample. The results confirmed uniform distribution of all elements; there were no visible regions with high content of particular elements and the absence of others. However, a closer examination of the SEM images of the samples with a higher Eu content revealed the presence of some plate-like particles. EDX mapping confirmed that these particles do not contain Sr, P, and Cl and can be attributed to Eu2O3 (Fig. S6). This type of particle was observed exclusively in samples containing the impurity phase and goes hand in hand with the results of XRD analysis. The oriented shape of Eu2O3 particles can explain the relatively high intensity of the impurity peaks in the XRD patterns due to preferred orientation (Fig. 1a).


image file: d5dt02634b-f2.tif
Fig. 2 SEM images of Sr5(PO4)3Cl:Eu powders containing 0.1 mol% (a), 0.25 mol% (b), and 2 mol% (c) of Eu; EDX mapping of Sr5(PO4)3Cl:0.25%Eu (d–i).

The phase conversion from starting Sr3(PO4)2:Eu to final Sr5(PO4)3Cl:Eu occurred in molten SrCl2, which provides a significant excess of the Sr2+ ions in the reaction medium. It is reasonable to suggest that Sr2+ ions compete with the Eu ions for the site occupancy in the crystal lattice of Sr5(PO4)3Cl during the crystallization process, which could lead to “wash out” and incomplete transfer of Eu from precursor to the product. Elemental analysis of Sr5(PO4)3Cl:Eu powders was performed by ICP-OES in order to determine the doping level experimentally. It should be noted that the Sr/P ratio in Sr3(PO4)2 and Sr5(PO4)3Cl is 1.5[thin space (1/6-em)]:[thin space (1/6-em)]1 and 1.67[thin space (1/6-em)]:[thin space (1/6-em)]1, respectively. Such a difference suggests that a fraction of Sr2+ ions required to form Sr5(PO4)3Cl is absorbed from the flux, since the amount of phosphate ions is fixed. The same behavior was previously demonstrated for converting amorphous calcium phosphate with a Ca/P ratio of 1.5[thin space (1/6-em)]:[thin space (1/6-em)]1 to Ca5(PO4)3Cl in molten KCl–CaCl2.38 The difference between the Sr/P ratio in the starting and final materials also reduces the percentage of Eu ions in the final material compared to the precursor, e.g., 1 mol% of Eu in Sr3(PO4)2 corresponds to 0.898 mol% in Sr5(PO4)3Cl. The ICP-OES analysis results (Table 1) indicate that the actual Eu content in the product is very close to the theoretical values, and the Eu loss in the form of Eu chloride or other water-soluble side-products during the phase conversion is insignificant. It is worth noting that ICP-OES provides the concentration of elements in the bulk material and does not prove the presence of all Eu ions in the Sr5(PO4)3Cl matrix. Moreover, the actual (Sr + Eu)/P ratio in Sr5(PO4)3Cl:Eu should be slightly lower than 1.67[thin space (1/6-em)]:[thin space (1/6-em)]1 due to the substitution of Sr2+ ions by aliovalent Eu3+, forming Sr2+ vacancies.

Table 1 Results of ICP-OES analysis of Sr5(PO4)3Cl:Eu powders
Nominal Eu content in Sr3(PO4)2:Eu (mol%) Nominal Eu content in Sr5(PO4)3Cl:Eu (mol%) Determined Eu content in Sr5(PO4)3Cl:Eu (mol%)
0.10 0.090 0.042
0.25 0.22 0.21
0.50 0.45 0.45
1.0 0.90 0.88
2.0 1.8 1.77


The PLE spectra of Sr5(PO4)3Cl:Eu samples for λem = 455 nm are shown in Fig. 3a. The observed spectra are typical of Eu2+ and consist of the broad bands with a maximum at approximately 270 nm. The highest intensity was observed for the sample doped with 0.25% Eu, while the lowest intensity was observed for the sample with the highest Eu content. The spectra of the samples with higher Eu content (1% and 2%) also demonstrate a slight decrease in intensity at 362 and 394 nm, which is associated with the typical excitation bands of Eu3+. This indicates the presence of Eu3+ ions and the co-existence of both oxidation states. The PL spectra of the samples excited at 270 nm (Fig. 3b) are dominated by a broad band centered at 445 nm, which is attributed to the [Xe]4f65d1 → [Xe]4f7 transition of Eu2+.2 The most intense emission was observed for the Sr5(PO4)3Cl:0.25%Eu sample, followed by a decrease in intensity with an increase in Eu content, possibly due to concentration quenching. The same effect at relatively low Eu2+ concentrations has been reported for Sr5(PO4)3Cl:Eu2+ in a previous work.40 The calculated FWHM values were 37 nm regardless of Eu content. While the PL spectra are dominated by Eu2+ emission, the emission of Eu3+ is also seen in the range from ca. 575 to 710 nm due to the overlap of the excitation spectra of Eu2+ and Eu3+ ions. The emission lines centered at around 591, 616, and 698 nm correspond to the 5D07F1, 5D07F2, and 5D07F4 intraconfigurational [Xe]4f6 → [Xe]4f6 transitions of Eu3+ ions, respectively.41 As seen, the Eu2+/Eu3+ emission intensity ratio decreased with an increase in Eu concentration. A possible reason is concentration quenching of the Eu2+ emission, whereas concentration quenching of Eu3+ was not achieved. Analogical observation for Sr5(PO4)3Cl:Eu2+/3+ system was previously reported by Chen et al.28 Moreover, a similar effect was observed for other Eu2+/Eu3+-containing inorganic matrices, including crystalline materials and glasses.42,43 The calculated QY values varied in the range from 6% to 42% being the highest for the sample with 0.1% of Eu and the lowest for 2% of Eu (Table S1).


image file: d5dt02634b-f3.tif
Fig. 3 PLE spectra (a); PL spectra. Inset: images of Sr5(PO4)3Cl:Eu under 254 nm irradiation (b); spectral deconvolution of the PL spectrum (c); normalized PL spectra under varying λex (d); normalized PL spectra under excitation wavelengths characteristic of Eu3+ (e); and decay curves (f) of Sr5(PO4)3Cl:Eu powders.

The shape of the emission band of Eu2+ is asymmetrical, suggesting the presence of Eu2+ ions in multiple crystallographic sites. The deconvolution of the PL spectrum with 2 Gaussian components resulted in good agreement between the cumulative fit and the experimental data (Fig. 3c). The presence of 2 sub-spectra centered at 21[thin space (1/6-em)]357 cm−1 (468 nm) and 22[thin space (1/6-em)]456 cm−1 (445 nm) correlates well with the crystal structure of Sr5(PO4)3Cl, having 2 inequivalent Sr sites.22

The emission of materials doped with mixed-valence Eu ions can be tuned by selecting a specific excitation wavelength. In some cases, this approach allows for the excitation of only one or both Eu species, resulting in the tunable emission.44,45 Moreover, this approach enables tuning of emission in materials where Eu2+ ions occupy multiple crystallographic sites.45Fig. 3d shows normalized PL spectra obtained under systematically varying excitation wavelength with a step of 10 nm. In our case, under a particular excitation wavelength, it was possible to eliminate the emission from Eu3+ species (e.g., 330–350 nm), whereas in general, the spectral changes were insignificant, as reflected in negligible Eu2+ emission band broadening and minor fluctuations in the Eu2+/Eu3+ emission ratio. As expected, such variations did not result in a perceptible shift of the CIE coordinates (Fig. S7).

The quantification of Eu2+ and Eu3+ in mixed-valence materials is challenging, especially in the case of low doping levels. A direct comparison of the emission intensities of Eu2+ and Eu3+ ions is unsuitable due to the different types of transitions that occur in these ions. Previously, for this purpose, Dereń et al. employed magnetic susceptibility measurements;46 however, we do not have the technical possibilities for such measurements. We also measured the PL spectra under the excitation wavelengths characteristic of Eu3+ to see if the Eu3+ emission could prevail. Fig. 3e demonstrates the PL spectra of the Sr5(PO4)3Cl:0.25%Eu sample under excitation at 361, 374, 380, and 393 nm. Evidently, a broadband emission of Eu2+ dominated the spectra in all cases, and the emission of Eu3+ in the 580–710 nm range constituted only 0.74%–2.9% of the entire emission, depending on the λex. This observation suggests that the majority of Eu ions exist in the reduced divalent state.

Fig. 3f shows the PL decay curves of Sr5(PO4)3Cl:Eu powders when the samples were excited at 405 nm, and the emission was monitored at 445 nm. The single-exponential decay model can be applied to the PL decay curves of all samples. The calculated PL lifetime values (τ) were independent of Eu content and varied only insignificantly from 527 to 534 ns, which is comparable with previously published data.40 Overall, it can be concluded that the room temperature photoluminescent properties of our synthesized materials agree well with those of Sr5(PO4)3Cl:Eu2+ prepared in a reducing atmosphere in terms of emission spectral shape, position, and PL lifetime values.22,40

The self-reduction of Eu in alkaline-earth metal phosphates is usually explained by the charge compensation model.7,28,47 According to this model, during the non-equivalent substitution in the crystal lattice, two Eu3+ ions replace three M2+ ions, which results in the simultaneous formation of two types of defects: (I) two EuM defects with a single positive charge and (II) one M2+ vacancy with a double negative charge to keep the neutrality of the material. These negatively charged vacancies act as electron donors, while positively charged Eu3+ defects act as electron acceptors. The interaction of the defects leads to the reduction of Eu3+ ions to the divalent state, which is further protected from the oxidizing air atmosphere by the phosphate framework. Such a mechanism can be reasonably suggested for the Sr5(PO4)3Cl:Eu system investigated in the present work and can be described by the following equations:

 
image file: d5dt02634b-t1.tif(1)
 
image file: d5dt02634b-t2.tif(2)
 
image file: d5dt02634b-t3.tif(3)

It is worth noting that some parallel processes related to the formation of oxygen defects can influence the degree of self-reduction.28,48,49 In the case of Sr5(PO4)3Cl, the formation of chlorine-related defects also cannot be excluded; however it needs further investigation.

The temperature-dependent luminescent properties of Sr5(PO4)3Cl:0.25%Eu in the 77–500 K range were further investigated (Fig. 4). The PLE spectra recorded at 77 K and 500 K at emission wavelength of 455 nm have the same shape with the maxima more expressed at low temperature (Fig. 4a). With an increase in the temperature the PL spectra demonstrated three trends associated with the intensity, emission maximum and FWHM values of the Eu2+-related emission (Fig. 4b). The intensity decreased with increasing temperature due to the thermal quenching. At 400 K, the integrated emission intensity constituted 73% and 87% of those at 77 and 300 K, respectively. In parallel, the linear increase in the FWHM values from 24 nm at 77 K to 47 nm at 450 K was observed (Fig. 4c). The emission maximum was stable at 449 nm in the temperature range from 77 to 150 K, followed by the gradual blue shift at higher temperatures down to 440 nm at 500 K. These results go hand in hand with the CIE 1931 chromaticity diagram (Fig. 4d), where color coordinates shift towards the center of the diagram with the temperature increase as a result of emission spectra broadening.


image file: d5dt02634b-f4.tif
Fig. 4 Temperature-dependent PLE spectra (a); PL spectra (inset – normalized PL spectra) (b); FWHM and normalized integrated intensity values (c); and CIE 1931 chromaticity coordinates (d) of Sr5(PO4)3Cl:0.25%Eu sample (λex = 270 nm).

It is evident that exposing Sr5(PO4)3Cl:Eu samples to ionizing radiation, such as X-rays or UV light, generates delocalized charge carriers that can become trapped in localized defect-induced energy levels within the band gap, known as charge traps. Charge traps temporarily capture and hold charge carriers, preventing them from recombining or conducting freely. The trap properties of materials are typically characterized by TSL measurements and analysis. Fig. 5a presents the TSL glow curves of the Sr5(PO4)3Cl:0.1%Eu sample after irradiation with X-rays and UV light. Regardless of the irradiation source, two distinct glow peaks are observed with Tmax values near 110 °C and 190 °C, indicating the presence of at least two types of charge traps. These two peaks were consistently detected across all studied samples (Fig. S8). In most cases, the number of discrete TSL peaks corresponds to the number of trap types in the material.50 The TSL emission spectra corresponding to both glow peaks exhibit the characteristic broadband blue luminescence of Eu2+, with no detectable emission from Eu3+. However, when the X-ray exposed sample is heated to 255 °C, Eu3+ luminescence bands around 600 and 700 nm appear (Fig. 5b). In contrast, the UV-irradiated sample shows no signs of Eu3+ emission, although it is worth noting that the overall luminescence intensity in this high-temperature range is significantly weaker than at the TSL peak temperatures. The differences could be explained by both the formation of X-ray-induced charge traps near Eu3+ or the partial ionization of Eu2+ to Eu3+ during the excitation.


image file: d5dt02634b-f5.tif
Fig. 5 TSL glow curves of the Sr5(PO4)3Cl:0.1%Eu sample after irradiation with X-rays or UV for 60 s (a); normalized TSL spectra of the Sr5(PO4)3Cl:0.1%Eu sample at different temperatures after irradiation with X-rays or UV (b).

For further investigation of trap properties, an X-ray irradiated Sr5(PO4)3Cl:0.1%Eu sample was selected. The widely recognized TmaxTstop and initial rise analysis (IRA) techniques were applied, and the results are illustrated in Fig. 6. These methods are analytical approaches in TSL used to determine the number of trap types and the activation energy (Ea) of charge traps in materials by examining how glow peaks shift under controlled preheating-cooling-TSL cycles. The methods are detailed elsewhere.51–53 As expected, the TmaxTstop plot (blue dots, Fig. 6c) indicates the presence of two types of traps. However, the determined Ea values (red squares, Fig. 6c) are less conclusive. The deep trap with Tmax = 190 °C is characterized as a discrete trap with an activation energy value of approximately 1.45 ± 0.10 eV. Meanwhile, the shallow trap with Tmax = 110 °C cannot be defined by a single Ea value and gradually varies from 0.93 to 1.34 eV with increased preheating temperature (Tstop). This suggests that the Tmax = 110 °C glow peak does not correspond to a discrete trapping site and is more likely associated with a quasi-continuous trap distribution. The appearance of trap distributions is anticipated in the case of the same type of trap in a highly disordered site.54,55 Although all obtained Ea values are somewhat deep, a persistent luminescence signal of Eu2+ can be detected for several hours after X-ray irradiation (Fig. S9).


image file: d5dt02634b-f6.tif
Fig. 6 TSL glow curves of the Sr5(PO4)3Cl:0.1%Eu sample after preheating to various Tstop values ranging from 30 to 240 °C in 10 °C increments, when the sample was irradiated with X-rays for 20 s before each preheating (a); IRA plots of the glow curves obtained from the TmaxTstop experiment (b), and TmaxTstop and EaTstop plots (c).

EPR spectra measurements were performed to gain additional insights into the charge trapping processes in Sr5(PO4)3Cl:Eu. As shown in Fig. 7a, paramagnetic radiation-induced radicals form upon X-ray irradiation. The EPR spectrum recorded at Q-band microwave frequency (Fig. 7b) highlights the anisotropy in signal shape, indicating anisotropy of the g-factor. The experimental spectra recorded at both microwave frequencies can be simulated using electronic spin S = 1/2 with g1 = 2.0038 ± 0.0005, g2 = 2.0018 ± 0.0005, and g3 = 1.9999 ± 0.0005. Various types of radicals in phosphate materials have been identified based on unpaired spin S interaction with magnetic 1H, 14N, or 31P nuclei.56–59 However, as no EPR spectrum hyperfine structure could be resolved in our case, such assignments are unlikely. The determined g-factor values are similar to those reported for CO2-type radicals in different hosts.59 It could be possible that a trace amount of carbon-containing impurities, such as carbonates, could lead to the formation of similar defects in Sr5(PO4)3Cl. Furthermore, thermal annealing in the 100–150 °C range (Fig. 7c) is correlated with the first peak observed in TSL glow curves (Fig. 5), which signifies the role of detected radicals in optical processes of the material.


image file: d5dt02634b-f7.tif
Fig. 7 Simulations of X-band (a) and Q-band (b) EPR spectra of the Sr5(PO4)3Cl:0.1%Eu sample after irradiation with X-rays; annealing kinetics of the X-ray induced radicals (c).

In summary, the molten salt synthesis offers a relatively simple route for the preparation of Eu2+-doped Sr5(PO4)3Cl, demonstrating an efficient Eu self-reduction. Although a limitation in terms of Eu doping level was observed, potentially it could be overcome by changing the flux composition by adding alkali metal chlorides, thereby reducing the percentage of SrCl2. The use of mixed flux in its turn could also lead to the synthesis of Sr5(PO4)3Cl:Eu2+ at significantly lower temperatures. Photoluminescent characteristics of the obtained materials were comparable to those of Sr5(PO4)3Cl:Eu2+ synthesized in a reducing atmosphere. The efficient Eu2+ emission, combined with slightly tunable photoluminescence and persistent luminescence, shows the potential of Sr5(PO4)3Cl for practical applications.

4. Conclusions

Sr5(PO4)3Cl:Eu2+ powders were successfully synthesized in an air atmosphere from Sr3(PO4)2:Eu3+ precursors. The phase transformation from Sr3(PO4)2:Eu to Sr5(PO4)3Cl:Eu was achieved in molten SrCl2 and accompanied by the self-reduction of Eu3+ to Eu2+. Although the PL spectra of the synthesis products were clearly dominated by the broadband emission characteristic of Eu2+, significantly weaker emission in the red region was also detected and ascribed to Eu3+, suggesting an incomplete Eu reduction. It was found that the Eu2+/Eu3+ emission intensity ratio decreased with an increase in Eu concentration. Overall, the photoluminescent properties of the synthesized materials agreed well with those reported in literature for Sr5(PO4)3Cl:Eu2+ prepared in a reducing atmosphere in terms of emission spectral shape, emission maximum, and the PL lifetime. The investigation of trap properties indicated the presence of two types of traps in the materials. Although all obtained Ea values were deep, a weak persistent luminescence signal of Eu2+ can be detected for several hours after X-ray irradiation. The results of EPR spectroscopy confirmed the formation of paramagnetic radiation-induced radicals and agreed well with the results of TSL.

Conflicts of interest

There are no conflicts to declare.

Data availability

The data supporting this study have been included within the article and the supplementary information (SI). Supplementary information is available. See DOI: https://doi.org/10.1039/d5dt02634b.

Acknowledgements

This project has received funding from the Research Council of Lithuania (LMTLT), agreement no. S-MIP-25-26. V. P. acknowledges LZP grant 2023/1-0063.

References

  1. S. Zhao, Y. Han, S. Lian and J. Zhang, Dalton Trans., 2025, 54, 8745–8763 Search PubMed.
  2. P. Dorenbos, J. Lumin., 2003, 104, 239–260 Search PubMed.
  3. Z. Yang, Y. Zhao, Y. Zhou, J. Qiao, Y.-C. Chuang, M. S. Molokeev and Z. Xia, Adv. Funct. Mater., 2022, 32, 2103927 CrossRef CAS.
  4. C. Dou, Z. Song and Q. Liu, J. Mater. Chem. C, 2024, 12, 11209–11241 RSC.
  5. J. Zou, L. Li, X. Fang, L. Chen and H. Guo, J. Mater. Chem. C, 2025, 13, 14808–14813 RSC.
  6. X. Lin, H. Han, M. Yang, Z. Yuan, Z. Chen, W.-G. Li, H. Kang, S. Zhang, Y. Zhang, Y.-X. Chen, T. Tian and H. Pang, Adv. Mater., 2025, 37, 2417420 CrossRef CAS PubMed.
  7. S. Khan, H.-W. Zheng, H. Jiao, S. Saleem, Z. Gul, J. Y. Al-Humaidi, A. A. Bahir, R. H. Althomali, A. Ali and M. M. Rahman, Rev. Inorg. Chem., 2024, 44, 547–567 CrossRef CAS.
  8. M. Peng, Z. Pei, G. Hong and Q. Su, J. Mater. Chem., 2003, 13, 1202–1205 Search PubMed.
  9. R.-K. Du, X.-L. He, T.-Z. Xiao, Y.-F. Xiang, L. Zhong, L. Zhou, J.-C. Zhang, D.-Q. Yao, T.-Y. Sun and M.-M. Wu, Laser Photonics Rev., 2025, 19, 2401211 Search PubMed.
  10. H. Yu, F. Ruan, L. Chen and D. Deng, Opt. Mater., 2020, 100, 109678 Search PubMed.
  11. W. Teng, H. Dong, C. Hu, X. Yang, J. Wang, X. Liang, B. Yang, J. Ru, B. Teng and D. Zhong, J. Lumin., 2024, 269, 120524 Search PubMed.
  12. R. Lu, X. Zhang, Y. Fang, X. Wu, M. Jia, K. Wang, J. Wu, Q. Li and Z. Sun, Laser Photonics Rev., 2024, 18, 2400409 Search PubMed.
  13. R. D. Shannon, Acta Crystallogr., Sect. A, 1976, 32, 751–767 CrossRef.
  14. M. Gu, W. Li, L. Jiang and X. Li, Acta Biomater., 2022, 148, 22–43 CrossRef CAS PubMed.
  15. M. Back, J. Cangiotti, J. Stadulis, A. Katelnikovas, M. G. Brik, P. Riello and A. Zarkov, Adv. Opt. Mater., 2025, e03109,  DOI:10.1002/adom.202503109.
  16. H.-S. Roh, S. Lee, F. Qin, S. Caliskan, C. Yoon and J.-K. Lee, ACS Appl. Nano Mater., 2018, 1, 4483–4490 CrossRef CAS.
  17. K. Szyszka, M. Kardach, D. Szymański and R. J. Wiglusz, J. Lumin., 2024, 275, 120788 CrossRef CAS.
  18. Y. Zhang, Z. Zhou and B. Mei, J. Eur. Ceram. Soc., 2024, 44, 5744–5751 CrossRef CAS.
  19. X. Liu, B. Mei and G. Tan, J. Eur. Ceram. Soc., 2024, 44, 4975–4984 CrossRef CAS.
  20. R. A. Talewar, S. Mahamuda, A. S. Rao, V. M. Gaikwad, P. D. Belsare and S. V. Moharil, J. Lumin., 2020, 222, 117118 CrossRef CAS.
  21. L. Fu, D. Wu, Y. Xiao, W. Zou, J. Kuang, Y. Liang, F. Du, J. Peng and X. Ye, J. Alloys Compd., 2021, 878, 160354 CrossRef CAS.
  22. D. Kim, S.-C. Kim, J.-S. Bae, S. Kim, S.-J. Kim and J.-C. Park, Inorg. Chem., 2016, 55, 8359–8370 CrossRef CAS PubMed.
  23. L. Zhou, H. Liang, P. A. Tanner, S. Zhang, D. Hou, C. Liu, Y. Tao, Y. Huang and L. Li, J. Mater. Chem. C, 2013, 1, 7155–7165 RSC.
  24. X. Chen, P. Dai, X. Zhang, C. Li, S. Lu, X. Wang, Y. Jia and Y. Liu, Inorg. Chem., 2014, 53, 3441–3448 CrossRef CAS PubMed.
  25. K. Liu, T. Wen, C. Li, Y. Ma, D. Jiang, B. Yue and Y. Wang, J. Mater. Chem. C, 2023, 11, 2162–2168 RSC.
  26. Z. Ma, S. Fang, Y. Bai, W. Wei and Z. Wang, Mater. Today Chem., 2024, 36, 101917 CrossRef CAS.
  27. Y. Deng, S. Yi, J. Huang, W. Zhao and X. Fang, J. Rare Earths, 2013, 31, 962–968 CrossRef CAS.
  28. J. Chen, Y. Liang, Y. Zhu, S. Liu, H. Li and W. Lei, J. Lumin., 2019, 214, 116569 CrossRef CAS.
  29. Y. Song, H. You, M. Yang, Y. Zheng, K. Liu, G. Jia, Y. Huang, L. Zhang and H. Zhang, Inorg. Chem., 2010, 49, 1674–1678 CrossRef CAS PubMed.
  30. H. Zou, M. Yan, G. Wang, B. Yuan, J. Huang, F. Gao, Y. Sheng, K. Zheng and Y. Song, Powder Technol., 2014, 254, 579–582 Search PubMed.
  31. L. Klimkeviciene, E. Parafjanovic, V. Klimkevicius and A. Katelnikovas, Ceram. Int., 2024, 50, 38456–38461 Search PubMed.
  32. S. Stoll and A. Schweiger, J. Magn. Reson., 2006, 178, 42–55 CrossRef CAS PubMed.
  33. M. Kemere, U. Rogulis and J. Sperga, J. Alloys Compd., 2018, 735, 1253–1261 CrossRef CAS.
  34. K. Szyszka, N. Nowak, R. M. Kowalski, J. Zukrowski and R. J. Wiglusz, J. Mater. Chem. C, 2022, 10, 9092–9105 Search PubMed.
  35. D. Karoblis, O. C. Stewart Jr., P. Glaser, S. E. El Jamal, A. Kizalaite, T. Murauskas, A. Zarkov, A. Kareiva and S. L. Stoll, Inorg. Chem., 2023, 62, 10635–10644 CrossRef CAS PubMed.
  36. S. L. Bennett, C. B. Finch, H. L. Yakel, J. Brynestad and G. W. Clark, J. Cryst. Growth, 1977, 41, 309–310 CrossRef CAS.
  37. B. O. Fowler, Inorg. Chem., 1974, 13, 194–207 Search PubMed.
  38. E. Kabasinskas, D. Karoblis, D. Griesiute, E. Raudonyte-Svirbutaviciene, S. Pazylbek, R. Lemezis, V. Klimavicius, A. Kareiva and A. Zarkov, Ceram. Int., 2024, 50, 16844–16851 Search PubMed.
  39. A. C. Taş, J. Am. Ceram. Soc., 2001, 84, 295–300 Search PubMed.
  40. J. Zheng, Q. Cheng, S. Wu, Z. Guo, Y. Zhuang, Y. Lu, Y. Li and C. Chen, J. Mater. Chem. C, 2015, 3, 11219–11227 RSC.
  41. Z. Hao, J. Zhang, X. Zhang and X. Wang, Opt. Mater., 2011, 33, 355–358 CrossRef CAS.
  42. X. Jiang, Y. Guo, L. Wang and Q. Zhang, Ceram. Int., 2023, 49, 28729–28740 CrossRef CAS.
  43. H. Chen, C. Zhou, X. Chen, C. Min, S. Lin, Y. Li, T. Zhou, J. Kang, C. Shi, C. Shao, P. Han, W. Strek, H. Chen and L. Zhang, J. Am. Ceram. Soc., 2025, 108, e20237 Search PubMed.
  44. B. Yu, Y. Li, Y. Wang, N. Li, P. Xiao, D. Liu and L. Geng, Inorg. Chem., 2022, 61, 2463–2475 CrossRef CAS PubMed.
  45. S. Pazylbek, J. Stadulis, G. Doke, A. Antuzevics, V. Pankratov, G. Merkininkaite, A. Katelnikovas and A. Zarkov, Dalton Trans., 2025, 54, 8625–8634 Search PubMed.
  46. P. J. Dereń, D. Stefańska, M. Ptak and P. Wiśniewski, J. Phys. Chem. C, 2021, 125, 24505–24514 Search PubMed.
  47. E. V. Sipina, D. A. Spassky, N. R. Krutyak, V. A. Morozov, E. S. Zhukovskaya, A. A. Belik, M. S. Manylov, B. I. Lazoryak and D. V. Deyneko, Materials, 2023, 16, 1383 CrossRef CAS PubMed.
  48. H. Li and Y. Wang, Inorg. Chem., 2017, 56, 10396–10403 Search PubMed.
  49. H. Wang, K. Su, L. Mei, Q. Guo and L. Liao, Inorg. Chem., 2023, 62, 12468–12479 CrossRef CAS PubMed.
  50. A. J. J. Bos, Radiat. Meas., 2006, 41, S45–S56 Search PubMed.
  51. S. W. S. McKeever, Phys. Status Solidi A, 1980, 62, 331–340 Search PubMed.
  52. V. Pagonis, G. Kitis and C. Furetta, Numerical and practical exercises in thermoluminescence, Springer New York, NY, 2006 Search PubMed.
  53. A. Antuzevics, G. Doke, G. Krieke, P. Rodionovs, D. Nilova, J. Cirulis, A. Fedotovs and U. Rogulis, Materials, 2023, 16, 1776 CrossRef CAS PubMed.
  54. K. Van den Eeckhout, A. J. J. Bos, D. Poelman and P. F. Smet, Phys. Rev. B: Condens. Matter Mater. Phys., 2013, 87, 045126 Search PubMed.
  55. G. Krieke, G. Doke, A. Antuzevics, R. Ignatans, I. Pudza and A. Kuzmin, J. Alloys Compd., 2023, 957, 170421 CrossRef CAS.
  56. D. V. Shurtakova, B. V. Yavkin, G. V. Mamin, S. B. Orlinskii, V. P. Sirotinkin, A. Y. Fedotov, A. Shinkarev, A. Antuzevics, I. V. Smirnov, V. I. Tovtin, E. E. Starostin, M. R. Gafurov and V. S. Komlev, Radiat. Res., 2020, 195, 200–210 Search PubMed , 211.
  57. A. Antuzevics, J. Cirulis, G. Krieke, D. Griesiute, A. Beganskiene, A. Kareiva, A. Dubauskas, V. Klimavicius and A. Zarkov, Mater. Chem. Phys., 2023, 310, 128479 Search PubMed.
  58. A. Antuzevics, G. Doke, G. Krieke, J. Stadulis, A. Beganskiene, A. Kareiva, C.-Y. Su, H.-W. Fang and A. Zarkov, J. Alloys Compd., 2025, 1012, 178525 CrossRef CAS.
  59. P. Fattibene and F. Callens, Appl. Radiat. Isot., 2010, 68, 2033–2116 Search PubMed.

This journal is © The Royal Society of Chemistry 2026
Click here to see how this site uses Cookies. View our privacy policy here.