Alexander
Mozalev
*a,
Maria
Bendova
a,
Lukas
Kalina
b,
Jan
Prasek
ac,
Francesc
Gispert-Guirado
d and
Eduard
Llobet
e
aDepartment of Microelectronics, Faculty of Electrical Engineering and Communication, Brno University of Technology, Technicka 10, 616 00 Brno, Czech Republic. E-mail: mozalev@vutbr.cz
bInstitute of Materials Science, Faculty of Chemistry, Brno University of Technology, Purkynova 118, 612 00 Brno, Czech Republic
cCEITEC – Central European Institute of Technology, Brno University of Technology, Purkynova 123, 61 200 Brno, Czech Republic
dSRCiT, University Rovira i Virgili, Av. Paisos Catalans 26, 43007 Tarragona, Catalonia, Spain
eMINOS, University Rovira i Virgili, Av. Paisos Catalans 26, 43007 Tarragona, Catalonia, Spain
First published on 27th May 2025
Nanostructured molybdenum oxide (MoOx) has many exciting properties that are highly dependent on the synthesis procedure. MoOx nanostructures should be aligned on a substrate for nanoelectronic on-chip applications, which has been challenging. Here, for the first time, arrays of MoOx-based nanoprotrusions of various morphologies (nanogoblets and nanorods), dimensions (20–500 nm), and surface densities (up to 1011 cm−2), spatially separated and vertically aligned on a Si wafer, were synthesized via self-organized porous-anodic-alumina (PAA)-assisted anodization of a Mo underlayer covered with a few nm thick Nb interlayer. This creative anodization approach enabled sustainable growth of fully amorphous MoOx within and under the PAA nanopores in several aqueous electrolytes, which other reported methods cannot accomplish. The nanoarrays grow via the outward migration of Mon+ cations enabled by the thin niobium-oxide interlayer, followed by the concurrent migration of Mon+ (n = 4–6) and Nb5+ cations in the PAA barrier layer and along the pore walls, competing with the migration of Mon+ through the anodic molybdenum oxide that grows within the ‘empty’ pores. The nanorods derived after selective PAA dissolution feature a core/shell heterostructure: The shells are composed of MoO3, several molybdenum suboxides (Mo5+, Mo4+), stoichiometric Nb2O5, and Al2O3, all mixed at the molecular level, whereas the cores are slightly hydrated and reduced MoO3, as revealed by X-ray photoelectron spectroscopy. The annealing in air or vacuum at 550 °C increases the oxidation state of Mon+ cations in the shells and causes the formation of monoclinic MoO2 and orthorhombic Nb2O5 nanocrystallites in the bottom oxide. Mott–Schottky analysis disclosed n-type semiconductor properties of the cores, with the charge carrier density reaching 1 × 1022 cm−3, whereas the shells seem more dielectric. The cyclic voltammetry and galvanostatic charge–discharge measurements featured characteristic reversible redox reactions, intensive electron transport, intercalation pseudocapacitive behavior, competitive charge-storage performance, and good rate capability of the rod's cores, which means the potential for nano-energy applications.
To fill the gap, we propose an alternative solution-based approach to synthesize multi-dimensional MoOx nanostructures highly ordered and vertically aligned on a substrate via smart anodizing of aluminum-on-molybdenum (Al/Mo) thin metal layers. The approach involves the growth of a porous anodic alumina (PAA) film immediately followed by anodizing the underlying Mo layer (hereafter ‘PAA-assisted anodizing’),13,14 all the electrochemical events occurring fully self-supportedly. The fundamental possibility of PAA-assisted anodizing was predicted theoretically and first justified experimentally by some of the present authors for Ti,15 Ta,16 and Nb.13 Even though PAA-assisted nanostructures have recently been synthesized on several more valve metals,17–21 there have been no reports on the PAA-assisted anodizing of Mo. The key challenge for preparing MoOx by electrochemical techniques is the oxide's instability and the formation of highly soluble complexes with a wide range of anions.22,23 This feature, complemented by oxide crystallization,24 transpassivity,25 suboxide formation tendency,26 slow cation migration rate,27 and an induction period revealed in anodic oxidation of Mo28 makes direct PAA-assisted growth on Mo extremely challenging.
It is assumed that the equilibrium between oxide formation and dissolution may be controlled by mixing molybdenum oxide with some other metal oxides during anodic-oxide growth. As an option, Al2O3–MoOx compounds might form due to the interaction of MoOx with the alumina barrier layer and PAA cell walls through the PAA-assisted anodizing of molybdenum. Moreover, binary strong-interacting nanostructured oxides could grow during the PAA-assisted anodizing of molybdenum laminated with a layer of a different valve metal forming miscible components. Depending on the relative migration rate of Mon+ ions in the mixture, even a minor addition of the second metal oxide might stabilize the composite.29
In the present work, we introduced a few-nm-thick interlayer of Nb between the Al and Mo layers, which were sputter-deposited onto a Si wafer. Such formed Al/Nb/Mo multilayer was anodized in several organic and inorganic acid electrolytes to tailor the balance between metal oxidation, oxide mixing, and oxide dissolution. Post-anodizing heat treatment was further employed to affect the composition, stoichiometry, and structure of the MoOx-based mixed oxides. The new nanoarrays were examined using high-resolution scanning electron microscopy, advanced surface and structure analysis techniques, and electrochemical measurements. A model of the PAA-assisted oxide growth was proposed, linking ionic transport and interfacial phenomena in the films to the electrical and electrolytic formation conditions. The applicability of the arrays as 3D nanoelectrodes for on-chip supercapacitors was explored and discussed.
Typically, the anodizing approach involved processing the Al overlayer in an aqueous acid solution to convert it into a PAA film, which was followed by the PAA-assisted re-anodizing of the Nb/Mo underlayers to a substantially higher voltage to achieve the growth of molybdenum and niobium anodic oxides within the PAA pores. Oxalic (H2C2O4), sulphuric (H2SO4), phosphoric (H3PO4), and more exotic malonic [CH2(COOH)2],31 tartaric [(CH(OH)(COOH))2],32 and etidronic [CH3C(OH)(PO3H2)2]33 acid solutions were probed as the anodizing electrolytes. The PAA layer formation was carried out galvanostatically at steady-state anodizing voltages ranging from 25 to 200 V, depending on the electrolyte. Selected samples were re-anodized to voltages relatively higher than the steady-state values established during the PAA growth in 0.5 M H3BO3 and 0.05 M Na7B4O7, pH 7.5 (hereafter, ‘borate buffer’). Finally, the PAA overlayers were dissolved in a chemical solution prepared and used as described elsewhere (hereafter, ‘selective etchant’),34,35 rinsed in ultrapure water, and dried in a cool nitrogen stream.
Following re-anodizing, selected samples were annealed at 550 °C for 3 hours either in ambient air at atmospheric pressure (hereafter ‘air-annealed’ samples) or at a residual pressure of 10−5 Pa (hereafter ‘vacuum-annealed’ samples).
X-ray photoelectron spectroscopy (XPS) analysis was conducted in a Kratos Axis Ultra DLD spectrometer and a Kratos Axis Supra spectrometer using a monochromatic Al Kα source with an X-ray emission power of 75 or 150 W and typical operating pressures less than 1.3 × 10−9 mbar. The X-ray beam was focused to a 300 μm × 700 μm spot. The emitted electrons were detected at fixed pass energies of 160 eV for the survey spectra and 20 eV for the high-resolution spectra. The Kratos charge neutralizer system was used for all measurements. The software for spectra analysis was CasaXPS version 2.3.17. GL(30) profiles were used for all components except the metallic core lines of Nb 3d, for which asymmetric profiles LA(1.2, 3.3, 12) were applied. All spectra have been charge-corrected to give the adventitious C 1s spectral component (C–C, C–H) binding energy of 284.8 eV. The quantitative analysis was performed from the high-resolution spectra using the relative sensitivity factors from CasaXPS suitable for Kratos Axis spectrometers, referenced to F 1s. Further details are described elsewhere.13,36,37
X-ray diffraction (XRD) patterns of the as-formed and annealed anodic films were taken from a Bruker-AXS D8-Discover diffractometer operated at 40 kV and 40 mA to generate CuKα radiation. An X-ray collimator of a 500 μm system was used. The VÅNTEC-500 detector (silicon strip technology, active area of 30 cm × 30 cm, frame size of 2048 pixels × 2048 pixels) was placed at a 15 cm distance from the sample. Sixteen frames were collected in reflection mode covering 20–90° 2θ with a step size of 0.8° to obtain a conventional 2D diffractogram suitable for Rietveld analysis.38 The exposure time was 300 s per frame, and it was γ-integrated to generate the 2θ vs. intensity diffractogram. The experimental diffractograms were fitted with the crystal structure39 for the phases identified using TOPAS 6.0 software (Bruker AXS GmbH, 2017).40
Electrochemical impedance spectroscopy (EIS), cyclic voltammetry (CV), and galvanostatic charge–discharge (GCD) measurements were carried out in the borate buffer at 22 °C using an Autolab PGSTAT204 Potentiostat/Galvanostat with a FRA32M module (Metrohm). A cylindrical PTFE cell secured the measured area of 0.25 cm2 for all electrochemical measurements. A three-electrode setup comprising the sample as the working electrode, an Au plate as the counter electrode, and an Ag/AgCl (1 M KCl) as the reference electrode was used in all measurements. The CV was typically performed between −1.9 and −0.1 V vs. Ag/AgCl with a scan rate of 50 mV s−1 starting from the open-circuit potential (OCP) of around −0.3 V vs. Ag/AgCl in the anodic direction to −0.1 V vs. Ag/AgCl, followed by one cathodic and one anodic sweeps. Experimental details of GCD, EIS, and Mott–Schottky measurements are given in the ESI.† Unless stated otherwise, all area-related physical quantities were related to the apparent surface area exposed to anodization or electrochemical measurements.
The PAA-assisted re-anodizing is carried out following a break to rinse and dry the pores after the anodizing. It is performed in the borate buffer galvanostatically under a low current density of 0.8 mA cm−2 until the re-anodizing voltage, Ur, reaches the set value (150 V), followed by a potential hold over 60 s (stage II). One may see that the voltage rise begins to retard at about 120 V. With reference to early works on compact anodizing of thin-film multilayers,45,46 it is assumed that the Nb interlayer is nearly fully transformed into anodic oxide and further anodizing consumes merely the Mo underlayer. The behavior appeared typical for all samples anodized in the oxalic acid and re-anodized up to the maximum voltage of 306 V (as shown in Fig. S1a and b†), at which dielectric breakdown interrupts the normal film growth. The Al(800 nm)/Nb(25 nm)/Mo(170 nm) trilayer anodized in the oxalic acid at Ust = 48 V to the end of stage I will be coded OX48; the same samples re-anodized to Ur = 150 V till the end of stage II will be coded OX48-150. The digit after the dash will change accordingly if the sample was re-anodized to a different final Ur value.
Fig. 1b shows an example of the voltage–time and current–time responses of the Al(800 nm)/Nb(15 nm)/Mo(170 nm) trilayer during galvanostatic anodizing in 0.2 M H2SO4 at 8.0 mA cm−2 followed by galvanostatic re-anodizing in the borate buffer at 0.8 mA cm−2 up to 105 V, both processes finishing with short potential holds. The anodizing responses show that the steady-state pore growth is established at 26 V, as one may expect for mild aluminum anodizing in 0.2 M H2SO4 at a low current density without initiating any specific effects.47 The re-anodizing voltage–time curve changes its slope at about 80 V, generally exhibiting the same tendency as in Fig. 1a. The lower voltage at which the slope changes is explained by the thinner Nb interlayer (15 vs. 25 nm). The Al(800 nm)/Nb(15 nm)/Mo(170 nm) trilayer anodized in the sulphuric acid at Ust = 26 V to the end of stage I will be coded SU26; the same samples re-anodized to Ur = 105 V till the end of stage II will be coded SU26-105. The schematics in Fig. 1 suggest preliminary views of the film structures expected at the end of the corresponding stages, which will later be updated based on SEM observations.
![]() | ||
Fig. 2 Surface, cross-sectional, and 3D SEM views of nanostructured anodic films made by (a–d) the anodizing of Al(800 nm)/Nb(25 nm)/Mo(170 nm) metal layers in 0.6 M oxalic acid at Ust = 48 V (coded as OX48, Fig. 1a) followed by (e–h) the re-anodizing in borate buffer to Ur = 180 V (coded as OX48-180, as in Fig. 1a). The images in (d, f, g and h) were recorded after dissolving the porous anodic alumina (PAA) layer in a selective etchant35 (PAA-free samples). |
The lower panel of Fig. 2 shows cross-sections and surfaces of the OX48-180 sample before and after the PAA dissolution. To an extent, the re-anodizing procedure lengthens the oxide protrusions inside the pores. An array of rod-like nanostructures rising to about 405 nm above the film surface, spatially separated and vertically aligned on the substrate, is derived after the PAA dissolution (Fig. 2f). As seen in Fig. 2f, the goblets' roots widen, and the bottom-oxide parts further expand into the underlying molybdenum metal, invading more space and forming nanoballs touching each other such that the balls form a continuous layer, 100 nm thick, buffering the protruding parts from the remaining Mo metal. In both samples (Fig. 2d and f–h), the measured population density of the protrusions is 8 × 109 cm−2, which corresponds well to the theoretical number of pores in the PAA overlayer. From the statistical analysis of the surface images of samples re-anodized to various voltages up to 220 V, the mean diameter of the rods is 50 nm regardless of the Ur-value, which is 1.7 times the average pore size in the PAA film (29 nm).
The definition and shifts of the principle interfaces in the OX48 and OX48-180 samples are elaborated in the cross-sectional SEM images in Fig. S2.† The development of the oxide nanorods and their bottom layers with increasing Ur is demonstrated in Fig. S3† with the help of frontal SEM views of the OX48-based samples re-anodized to various Ur ranging from 150 to 220 V. The lines drawn over the images indicate the depths of the bottom layers and the rods' lengths within the pores. The SEM observations and measurements for the OX48-based samples shown in Fig. 2 and S2, S3,† complemented by the XPS and XRD data analyses, create the basis for understanding the ionic transport and mechanism of oxide growth, which will be discussed in Section 3.1.5.
Several other organic and inorganic acid electrolytes, commonly or rarely used for PAA formation, have also been tried in this work, with the best results achieved to date in 0.2 M H2SO4 and 0.2 M H3PO4 aqueous solutions. Fig. 3 shows selected SEM images of cross fractures and surfaces before and after PAA dissolution of the Al/Nb/Mo multilayers anodized/re-anodized in 0.2 M sulphuric acid/borate buffer (sample SU26-105) and 0.2 M phosphoric acid at Ust = 150 V following the anodizing approach described in our previous works (Fig. S1c†).17,50 In the case of sulphuric-acid anodizing, the thickness of the Nb interlayer was 15 nm to involve molybdenum in the oxidation process more substantially. From SEM observation of the SU26-105 sample (Fig. 3a–c), the PAA-assisted anodizing generates arrays of tiny rod-like nanostructures of the highest population density of 3 × 1010 cm−2, about 20 nm wide, 220 nm long, and supported by an array of semispherical bottom-oxide regions in the remaining Mo metal layer. Alternatively, the goblet-like protrusions generated via the PAA-assisted anodizing/re-anodizing in the phosphoric acid (Fig. 3d–f) appear proportionally bigger, exhibiting the lowest population density of 7 × 108 cm−2. The mean center-to-center distance of 400 nm measured in this sample is the longest achieved by the approach developed in this work.
![]() | ||
Fig. 3 Surface and cross-sectional SEM views of nanostructured anodic films made by (a–c) the anodizing of Al(800 nm)/Nb(15 nm)/Mo(170 nm) metal layers in 0.2 M sulphuric acid at Ust = 26 V followed by the re-anodizing in the borate buffer to Ur = 105 V, as in Fig. 1b, and (d–f) the anodizing of Al(800 nm)/Nb(25 nm)/Mo(170 nm) metal layers in 0.2 M phosphoric acid at Ust = 150 V followed by re-anodizing to Ur = 160 V, as shown in Fig. S1c.† The images in (b, c, e and f) were recorded after dissolving the PAA layers in the selective etchant (PAA-free samples). The unlabelled scale bars are 200 nm. |
Based on the SEM examination of various samples, we selected the nanoarrays synthesized in the oxalic acid (the OX48-based films) as model systems for carrying out chemical and structural analyses and investigating the cooperative ionic transport during the PAA-assisted oxide growth on the superimposed Nb and Mo thin film layers.
![]() | ||
Fig. 4 Experimental and curve-fitted narrow-scan (left column) Mo 3d, (middle) Nb 3d, and (right) Al 2p XP spectra of the (a–c) OX48, (d–f) OX48-220, (g–i) air-annealed OX48-220, and (j–l) vacuum-annealed OX48-220 samples. The sample codes and formation conditions are defined in Fig. 1 and 2. The PAA layers were dissolved in the selective etchant before the XPS analysis. The peak positions, FWHMs, and at% are summarized in Table S1.† |
![]() | ||
Fig. 5 (a) Schematics and (b and c) experimental and curve-fitted narrow-scan (b) Mo 3d and (c) Al 2p XP spectra of the vacuum-annealed PAA-inbuilt OX48-220 sample. |
Narrow-scan C 1s, O 1s, Mo 3d, Nb 3d, and Al 2p spectra were collected to analyze the elements' core levels and bonding states. The experimental and fitted Mo 3d, Nb 3d, and Al 2p spectra of selected OX48-220-based films are shown in Fig. 4 and 5. Spectra of the other samples are presented in the ESI† (PAA-free OX48-180, PAA-free OX48-15 nm Nb-based, and PAA-half-etched OX48-220-based films, Fig. S5 and S6†), including the details of deconvoluting the Mo 3d spectra, also considering the Nb 3d loss peaks partially overlapping with the Mo 3d transitions (Fig. S4†).
The analysis of Mo 3d spectra of all the OX48-based films (left columns in Fig. 4 and S5, S6†) was complicated by a substantial contribution of Nb 3d loss peaks partially overlapping with the Mo 3d transitions because the Mo:
Nb ratio was relatively low (<25 at% Mo, provided that at%(Nb + Mo) = 100 at%). The detailed procedure of adding Nb 3d loss peaks while maintaining a constant Nb-3d-loss-to-Nb-3d ratio of 0.175 ± 0.02 is described in the ESI.† The Mo 3d transitions are fitted with 3d5/2–3d3/2 doublets with a constrained spin–orbit splitting of 3.13 eV, fixed intensity ratio 3d5/2
:
3d3/2 of 3
:
2, and a full width at half maximum (FWHM) equal for 3d5/2 and 3d3/2 components.
Up to four Mo 3d doublets reproduce each spectrum, with Mo 3d5/2 at 232.4 ± 0.2, 231.0 ± 0.2, 229.6 ± 0.2, and 234.3 ± 0.2 eV, with variable individual contributions to each spectrum. Based on the literature reports,51–53 we assign the doublet at 232.4 eV (Mo 3d5/2) to Mo6+ cations in MoO3. The lowest-binding-energy (BE) doublet at 229.6 eV (Mo 3d5/2) is assigned to Mo4+ cations in MoO2. The highest-BE doublet at 234.3 eV (Mo 3d5/2), identified in the spectra of the as-prepared films, is associated with Mo6+–OH(H2O) coordination. Last, the doublet at 231.0 eV (Mo 3d5/2) may be assigned to Mo5+ cations in Mo2O5. The various oxides are assumed to be mixed at the molecular level, which may be expressed as MoVIy1MoVy2MoIVy3Ox1(OH)x2 and vary in the different parts of the anodic films, such as the rods and the bottom oxide.
The dissimilarities in the recorded Mo 3d spectra of the PAA-free films reflect the differences in the content of the individual Mon+ species. Three characteristic types of MoOx (marked in Fig. 4d, g and j) can be distinguished: type I – ‘highly reduced’ MoOx, which comprises a dominating amount of Mo4+ cations, is characteristic of the re-anodized as-prepared films (Fig. 4d, left column in Fig. S5†). Type II – ‘moderately reduced’ MoOx, which comprises Mo6+, Mo5+, and Mo4+ cations in comparable concentrations, is associated with the air-annealed film (Fig. 4g). Type III – ‘slightly reduced’ MoOx, which contains a dominating amount of Mo6+ cations, is linked to the vacuum-annealed film (Fig. 4j and 5b). The average values of oxidation state for Mo ions in the oxide types are 4.73 ± 0.1 (type I, six samples), 4.98 ± 0.1 (type II, four samples), and 5.40 ± 0.1 (type III, six samples), beside the vacuum-annealed PAA-inbuilt film, which revealed the presence of almost pure MoO3 (Fig. 5b).
The Mo 3d pattern of the PAA-free OX48 sample (Fig. 4a) cannot be analyzed precisely because of a low Mo content (4.2 at%, providing that at%(Nb + Mo) = 100%, calculated after subtracting the metallic contributions from the Nb 3d spectrum, as will be shown later). The PAA-free OX48-220 sample, which is a reference for comparison with the other samples, comprises type I MoOx (Fig. 4d). Re-anodizing to a relatively low Ur = 180 V (OX48-180) or employing a thinner (15 nm) Nb interlayer in the Al/Nb/Mo trilayer (coded as OX48-220-15 nm Nb) does not alter the MoOx pattern (left column in Fig. S5†). However, when the half-etched PAA covers the roots of the OX48-220 nanorods and the bottom oxide, type II MoOx is revealed (Fig. S6a†). Since the bottom oxide is unreachable for the XPS analysis in the PAA-half-etched sample and only the rods emit photoelectrons, the nanorods' outer layer is assumed to be more oxidized than the bottom oxide. Moreover, all re-anodized OX48-based samples contain 5–10% of hydroxylated MoO3, which may be expressed as MoO3−x(OH)2x.
The quantitative analysis shows that Mo content in the four various re-anodized PAA-free OX48-based films (see Table 1 and left column of Fig. S5†) ranges between 11.5 and 15.5 at% (provided that at%(Nb + Mo) = 100%). It increases slightly with increasing re-anodizing voltage or thinning Nb interlayer. The PAA-half-etched OX48-220 surface reveals a substantially higher Mo content of 19.3 at%, assuming compositional differences in the various film parts, with more molybdenum oxide in the rods' surface than in the bottom oxide.
Film code | State of PAA dissolution | Mo content (at%) (at%(Nb + Mo) = 100 at%) | Average ox. state of Mo/type | Amount of Nbn+ (n = 3 and/or 4) (%) | Al content (at%) (at%(Al + Nb + Mo) = 100 at%) | Figure |
---|---|---|---|---|---|---|
OX48 | PAA-free | 4.2 | 5.45/? | 5.3 | 24 | Fig. 4a–c |
OX48-180 | PAA-free | 11.5 | 4.81/I | 2.1 | 56 | Fig. S5a–c |
OX48-220 | PAA-free | 14.1 | 4.67/I | 3.2 | 54 | Fig. 4d–f and S5d–f, S6d–f |
PAA-half-etched | 19.3 | 5.13/II | 0 | 97 | Fig. S6a–c | |
OX48-180-15 nm Nb | PAA-free | 12.6 | 4.63/I | 5.2 | 54 | Fig. S5g–i |
OX48-220-15 nm Nb | PAA-free | 15.5 | 4.88/I | 2.1 | 51 | Fig. S5j–l |
Air-annealed OX48-220 | PAA-free | 18.3 | 5.00/II | 1.9 | 60 | Fig. 4g–i and S6j–l |
PAA-half-etched | 22.4 | 5.39/III | 0 | 85 | Fig. S6g–i | |
Vacuum-annealed OX48-220 | PAA-free | 22.9 | 5.49/III | 0.7 | 42 | Fig. 4j–l |
PAA-inbuilt | 100 | 5.85/III | n/a | 96 | Fig. 5b and c |
Comparative analysis of Mo 3d spectra of the PAA-free air- and vacuum-annealed OX48-220 films (Fig. 4g, j and Table 1) assumes that MoOx is more oxidized in the annealed films (type II and III) than in the as-prepared film (Fig. 4d, type I). Furthermore, the highest degree of MoOx oxidation (type III) is noted in the vacuum-annealed sample. The two annealed films also show higher Mo content than the as-prepared sample. The air-annealed PAA-half-etched sample (Fig. S6g†), where only the rods are PAA-free, not the bottom layer, reveals relatively more oxidized MoOx and a higher overall Mo content compared with its PAA-free counterpart (Fig. 4g). Furthermore, the air and vacuum-annealed films do not contain MoO3−x(OH)2x.
The most stunning effect is noted in the vacuum-annealed PAA-inbuilt sample, in which only the rods' tops and the PAA surface emitted photoelectrons, as shown in Fig. 5a. Here, 100 at% Mo is associated with slightly reduced and hydrated MoO3, assuming that the entire inner oxide composing the rods is MoOx with no additions of Nb2O5. The inner oxide comprises a small amount of MoO3−x(OH)2x, which cannot be detected when the whole surface of the PAA-free films is exposed to the analysis.
The location of various types of MoOx and the differences in the overall Mo content (when at%(Nb + Mo) = 100%) over the various parts of the OX48-220 samples (as-prepared, air-annealed, and vacuum-annealed) are depicted in Fig. 6.
![]() | ||
Fig. 6 Schematic cross-sectional views visualizing the XPS and XRD results for the (a) as-prepared (as in Fig. 1 and 2), (b) air-annealed (550 °C, 3 h, atmospheric pressure), and (c) vacuum-annealed (550 °C, 3 h, 10−5 Pa) OX48-220 samples. |
To summarize the Mo 3d peak analysis, the surface of the oxide nanorods comprises relatively more oxidized MoOx (type II or III, about 20 at% Mo), whereas the bottom-oxide's surface contains less-oxidized MoOx, most likely MoO2 (about 5 at% Mo), and is enriched with Nb2O5. The oxide composing the nanoballs of the bottom layer (Fig. 6) contains no niobium oxide but reduced MoOx, likely MoO2. The interior of the rods is slightly reduced MoO3 mixed with a minor amount of MoO3−x(OH)2x without any addition of Nb2O5.
The Nb 3d spectra of all OX48-based films (middle columns in Fig. 4 and S5, S6†) are fitted with Nb 3d5/2-3d3/2 doublets with a constrained spin–orbit splitting of 2.75 eV, fixed intensity ratio 3d5/2:
3d3/2 of 3
:
2, and a FWHM equal for the 3d5/2 and 3d3/2 components. All the spectra contain a dominant doublet with Nb 3d5/2 component at 207.18 ± 0.15 eV, associated with Nb5+ cations in Nb2O5.13,36,49 For most of the films, several low-intensity doublets are added with Nb 3d5/2 at 205.54 ± 0.15, 204.25 ± 0.2, 202.2 ± 0.3, and 208.03 ± 0.1 eV, which are assigned to Nb4+, Nb3+, Nb0, and Nb5+–OH/H2O coordinations, respectively.13,36,49 Thus, the surface of the PAA-free OX48 film (Fig. 4b) contains a dominating amount of Nb2O5 mixed at the molecular level with a minor amount (5%) of Nb4+- and Nb3+-based suboxides, while some metallic residues remain between the bases of the nanoprotrusions (Nb0 and Nb2+ cations, ∼20% of all Nb species in the spectrum). Notably, the metallic Mo0 peak is not present in the corresponding Mo 3d spectrum (Fig. 4a) because the unoxidized Mo is buried under the residues of the 25 nm thick Nb network. The four PAA-free OX48-based films, made by re-anodizing the Al/Nb(25 nm)/Mo or Al/Nb(15 nm)/Mo trilayers to 180 or 220 V (Fig. 4e, middle column in Fig. S5†), also contain Nb2O5 mixed with a low amount of suboxides (2–5%, a summary is available in Table 1). A minor amount of metallic niobium (0.5–7%), further decreasing with increasing re-anodizing voltage, is noted. A substantial change is observed for the PAA-half-etched OX48-220 film (Fig. S6b†), where the rods emit photoelectrons but not the bottom oxide. This surface features the presence of stoichiometric Nb2O5 and the absence of metallic residues. This means that the Nb suboxides detected in the PAA-free films reside in the bottom-oxide layer, not in the rods, and the remaining PAA layer masks the metallic residues.
The PAA-free air- and vacuum-annealed OX48-220 samples (Fig. 4h and k), similarly to their as-prepared counterpart (Fig. 4e), contain a dominating amount of Nb2O5 mixed with NbO2 and Nb2O3 (<2 at%). There are no metallic Nb0 peaks in the spectra. Considerable amounts of hydroxylated Nb2O5 are present in the annealed films, with Nb5+–OH/H2O coordination of ∼7%, which can be expressed as Nb2O5−x(OH)2x. Therefore, the two annealed surfaces become more oxidized. Paradoxically, the vacuum-annealed surface appears more oxidized than the air-annealed one, which agrees with the trend observed for the MoOx. When the half-etched PAA covers the bottom oxide in the air-annealed film, the Nb 3d spectrum (Fig. S6h†) has no suboxide peaks, meaning that the suboxides reside in the bottom oxide, not in the rods, similar to the as-prepared sample. However, the Nb5+–OH/H2O coordination (6%) is identified in the Nb 3d spectrum of the air-annealed PAA-half-etched sample in a larger amount than in the PAA-free sample (4%). This implies that the rods' surface accommodates hydroxylated Nb2O5, not the bottom oxide.
The Al 2p spectra of the OX48-based samples (right columns in Fig. 4 and S5, S6†) are relatively simple and are all fitted with up to three symmetrical peaks associated with Al2O3 (74.63 ± 0.3 eV, dominating amount), Al0 (72.08 ± 0.05 eV), and Al3+–OH (76.00 ± 0.15 eV). The surface layer of the PAA-free OX48 (Fig. 4c) contains ∼30 at% Al0, in addition to Al2O3. The presence of metallic Al is due to the network of non-anodized aluminum around the oxide nanoprotrusions. The Nb0 doublet in the corresponding Nb 3d spectrum has the same origin (Fig. 4b). The metallic contributions to the Nb 3d and Al 2p spectra were subtracted from the overall content of the elements to obtain an approximate surface concentration of Al3+ in the anodic parts of the film. The corresponding native alumina, covering the Al0 network, was also considered and subtracted.54 Provided that at%(Al + Nb + Mo) = 100%, the surface of the oxide nanorods in the anodized sample contains 24 at% Al (Al3+).
The Al 2p spectra of the four PAA-free as-reanodized OX48-based films (Fig. 4f, right column in Fig. S5†) contain the three peaks associated with a dominating amount of Al2O3 and minor amounts of Al3+–OH coordination (10–15 at%) and Al0 (1–5 at%). The contribution of Al0 decreases with increasing re-anodizing voltage from 180 to 220 V. The amount of Al in the surface layer of the PAA-free as-reanodized films is 50–55 at% (when at%(Al + Nb + Mo) = 100%). This finding agrees with previous reports on several PAA-assisted nanostructures (N-doped TiO2,55 Se-doped Nb2O5,49 and Se-doped ZrO2)35 containing 50 to 80 at% Al in the form of Al2O3.
The PAA-half-etched OX48-220 sample (Fig. S6c†) ontains Al2O3 only. The Al0 peak is absent in the spectrum since the underetched PAA covers the aluminum residues. The absence of Al3+–OH coordination implies that the hydroxylated Al2O3 resides in the rods' roots. The deep-laid bottom oxide is supposed to be alumina-free because it forms merely by the inward migration of O2− anions.
The Al 2p spectra of the PAA-free annealed OX48-220 films (Fig. 4i and l) also contain the Al3+–OH peak (∼13 at%), while its presence in the vacuum-annealed sample spectrum is uncertain. The air-annealed film contains Al0 residues in the same amount as the corresponding as-reanodized film, while the vacuum-annealed film is Al0-free. The amount of Al in the surface layer of the PAA-free annealed films is 40–60 at% (when at%(Al + Nb + Mo) = 100%), which is similar to the as-prepared films. The PAA-half-etched air-annealed sample (Fig. S6i†) does not have Al3+–OH coordination, which indicates that the hydroxylated alumina resides in the rods' roots. On the other hand, the Al 2p spectrum of the PAA-inbuilt vacuum-annealed film (Fig. 5c) has an intense peak attributed to the Al3+–OH coordination (18 at%).
Summarizing the XPS analysis results, the surface layers of the nanoarrays prepared in this study comprise stoichiometric MoO3, molybdenum suboxides (Mo5+ and Mo4+), stoichiometric Nb2O5, niobium suboxides (Nb4+ and Nb3+), and Al2O3, distributed as depicted in Fig. 6 and mixed at the molecular level. The inner part of the rods is a slightly reduced pure MoO3. The overall surface content of Mo increases up to 23 at% with increasing re-anodizing voltage, thinning the Nb interlayer, and annealing the films at 550 °C.
![]() | ||
Fig. 7 Comparative X-ray diffractograms for the (1) OX48, (2) OX48-180, (3) OX48-220, (4) vacuum-annealed OX48-220, and (5) air-annealed OX48-220 samples. |
The diffractograms of all the samples are interpreted with the presence of a polycrystalline metallic Mo phase (Imm space group, crystallite size of 20 to 30 nm), which reveals a preferred orientation growth along 〈110〉 direction and is associated with a layer of unoxidized Mo. Since the intensities of the dominating (110) Mo peaks in the diffractograms of the re-anodized, vacuum-annealed, and air-annealed samples are comparable, it is assumed that the thickness of the remaining Mo underlayer is not affected by the 550 °C annealing. This may be explained by the thick anodic oxides above the Mo metal obstructing oxygen diffusion under the chosen annealing conditions.
Another feature is that the anodized OX48 sample contains Al and Nb metals. This agrees with the SEM and XPS results for OX48. From the OX48-180 sample's diffractogram, it is assumed that the Al metal is fully consumed while the residues of the Nb metal network remain on the sample surface. Since (110) Nb peak disappears from the diffractogram of the OX48-220 sample, the Nb metal becomes fully oxidized at Ur > 180 V. The absence of any oxide phases in the as-anodized and re-anodized samples confirms that the electrochemically grown oxides are entirely amorphous.
Contrarily, the annealed OX48-220 films contain well-identified nanocrystalline monoclinic MoO2 phase (P21/c space group, crystallite size ∼19 nm) in the amount of 24 wt% in the vacuum-annealed sample and 33 wt% in the air-annealed sample. Additionally, the air-annealed sample contains ∼5 wt% orthorhombic Nb2O5 nanocrystallites (Pbam space group). The MoO2 nanocrystallites grow with a preferred orientation along 〈21〉 direction whereas the Nb2O5 nanocrystallites are highly oriented along 〈001〉 and 〈100〉 directions. The Nb2O5 phase is also present in the vacuum-annealed sample in a minor amount, which makes it difficult to estimate the crystallite size reliably.
The more considerable total amount of crystalline oxides in the air-annealed OX48-220 sample relative to the vacuum-annealed sample (∼38 vs. ∼26 wt%) implies that a bigger portion of initially amorphous anodic oxides crystallizes due to the heating in air.
![]() | ||
Fig. 8 SEM images of fragments of cross-fractures of the OX48-180 sample disclosing a core/shell heterostructure of the oxide nanorods and uneven composition of the bottom-oxide layer. |
![]() | ||
Fig. 9 Schematic model of film growth: (a) the deposition of an Al/Nb/Mo trilayer, (b) the porous anodizing of aluminum in 0.6 M oxalic acid at Ust = 48 V, (c) the beginning of niobium oxidation, (d) the end of the anodizing stage I as in Fig. 1a, (e) the re-anodizing to 150 V to grow mixed-oxide nanorods, (f and g) the re-anodizing to respectively 180 and 220 V to extend the rods in the pores, (h) the selective PAA dissolution. The lower panel shows the surface fragments corresponding to the upper cross-sections after an imaginary dissolution of the PAA overlayer. The dotted line across the surface fragments shows the position of the imaginary section plane. The colors differentiate the oxides and component concentrations, as the legends show. |
According to the model, the sputter-deposited Al/Nb/Mo trilayer on a SiO2/Si wafer (Fig. 9a) is anodized (Fig. 9b) until the underlying Nb is reached (Fig. 9c). The nucleation and growth of niobium-oxide nanostructures under the pores till the end of stage I is described in detail in our previous publication and may be inherited for the present case.13 The difference, however, is that the thickness of the Nb interlayer is insufficient to preserve the underlying Mo from anodic oxidation. In other words, molybdenum anodizing starts already during the current decay at stage I, and Mon+ cations begin to migrate outwards once the anodizing front touches the Mo underlayer. Therefore, the nanogoblets in Fig. 9d contain molybdenum oxides mixed with niobium oxides and alumina originating from the PAA barrier layer. The end of stage I features the residues of the Al/Nb bilayer in the form of a continuous network surrounding the goblets. The mechanism for forming such a network is based on the relation between the ionic resistances of the anodic alumina and niobia, as described in detail elsewhere.13,35
During the re-anodizing (stage II), the remaining Al/Nb network is gradually consumed, while the Mo layer is further oxidized and the rods grow steadily within the pores. The Al/Nb consumption competes with further molybdenum oxidation until neighboring molybdenum-oxide areas incorporated into the metal expand and merge to form a relatively uniform bottom layer, though having a wavy profile at the MoOx/Mo interface even at the final re-anodizing voltage of 220 V. The shells of the rods form due to the simultaneous migration of Mon+ (n = 4–6) and Nb5+ cations in the outer part of the pore walls, which are more defective, less dense, and contaminated by electrolyte-derived species, such as C2O42− in the case of oxalic-acid anodizing.56 During the upward oxide growth, the alumina partially dissolves from the outmost surface of the pore walls.57 The degree of such dissolution impacts the amount of alumina that becomes included in the shell composition and remains after the PAA dissolution. Thus, the shells of the rods derived after the PAA dissolution are composed of various molybdenum oxides (Mo6+, Mo5+, Mo4+), stoichiometric Nb2O5, and Al2O3, all mixed at the molecular level.
In contrast with the shells, the cores are pure molybdenum oxide, which grows without mixing with niobium oxide and does not include alumina because it forms inside the pores without interacting with the pore walls. The absence of niobium oxide in the core composition is explained by the prevalent migration of Nb5+ within the shells and by the shortage of niobium supply from the 25 nm thick Nb interlayer (see also the quantitative analysis presented in the ESI† file). Within the core, MoO3 (dominating amount) is mixed at the molecular level with minor amounts of oxide-hydroxide MoO3−x(OH)2x and molybdenum suboxide Mo2O5, which reminds the case of anodizing an Al/W couple.17,58 The electronic properties of the cores/shells heterostructures will be discussed in Section 3.2.
The thin oxide layer, shown as a pink strip (upper row of Fig. 9) and pink circles (lower row of Fig. 9) covering the deep-laying part of the bottom layer, is a reduced NbOx (dominating amount) mixed with a minor amount of MoO2. The innermost anodic oxide composing the semi-balls, balls, and merging balls (Fig. 9) is pure molybdenum suboxide, likely MoO2, free from niobium-oxide contamination. This is because the oxide within the balls is formed exclusively via the migration of O2− (OH−) from the electrolyte through the NbOx interlayer, which resides above the Mo layer and has a physically sharp interface.
The last formation step shown in panel (h) is the PAA dissolution. It can be managed selectively toward the nanorods, an excellent achievement of our work. The rods survive the treatment because the multicomponent shell composition prevents the molybdenum anodic oxides from chemical dissolution.
2MoO2 + O2 → 2MoO3 | (1) |
2Mo2O5 + O2 → 4MoO3 | (2) |
Along with similar crystallization effects, the paradoxical increase in the amount of MoO3 in the rods' shell of the vacuum-annealed OX48-220 film (Fig. 4j), exceeding that in the air-annealed film (Fig. 4g), may be caused by irreversible heat-enabled diffusion of niobium cations away from Nb2O5 in the rods' shells, driven by a concentration gradient in the oxygen-deficient atmosphere (as depicted in Fig. 6c), i.e., at circumstances when oxygen uptake is impossible.22 Such a prevalent disruption of Nb2O5 in the mixed niobium–molybdenum oxides seems reasonable because the bond energy of O–Nb (328 kJ mol−1)60 is lower than that of O–Mo (359 kJ mol−1).27 The released oxygen anions oxidize the molybdenum suboxide(s), thus increasing the oxidation state of MoOx in the shells. The released Nb5+ cations likely diffuse into the cores, increasing the Mo/Nb ratio in the shells (Fig. 6c). The lowering of Nb (increasing of Mo) amount in the shells due to the vacuum annealing agrees well with the XPS analysis results summarized in Fig. 6c. Such an impact of vacuum annealing is unique since it has not been reported for any nanostructured oxides made via the PAA-assisted anodizing of valve metals.61
The vacuum annealing does not cause lattice expansion of the Mo metal phase, which means the oxygen species do not diffuse from the oxide into the interstitial sites of the remaining Mo metal.22 It is thermodynamically possible that the oxide within the nanoballs in the bottom layer reacts with the substrate metal, causing the loss of oxygen from the deep-laying MoO2.23 Even if this is also likely kinetically, the effect is too minor to be detected by XRD and has no relation to the oxides composing the cores and the shells.
![]() | ||
Fig. 10 (a) CV curves (scan rate 50 mV s−1) in the borate buffer solution for the PAA-inbuilt OX48-180 sample. (b) Capacity values calculated from the CV curves and from a comparable galvanostatic charge–discharge (GCD) curve (shown in Fig. S12†), having similar charging times of 36 and 60 s, respectively; the potential range was −0.1 to −1.9 V vs. Ag/AgCl. The quantities were related to the apparent (Aa) and effective (Ae) surface areas; Ae = 0.1 × Aa. |
The level of CV current density (∼0.1 mA cm−2, Fig. 10a, right y-axis), compared with the literature reports (∼10 mA cm−2 at 50 mV s−1),7,62 seems low. On the other hand, in the PAA-inbuilt sample, only about 10% of the apparent surface area (Aa) interacts with the electrolyte, as shown in the embedded schematics in Fig. 10a. Therefore, to judge the actual performance of the material, we relate the CV current density to the effective surface area (Ae), left y-axis in Fig. 10a, i.e., as if the measured surface would be a flat MoOx, then it would reach 1 mA cm−2. Furthermore, using Ae, we calculate the areal capacities from the CV curves (Fig. 10b, the calculations are available in the ESI, Fig. S11†), and the charging capacity of 4.1 μA h cm−2 is obtained, which is higher than the discharging capacity (3.1 μA h cm−2), and lower than a charging capacity obtained from the GCD curves (10.2 μA h cm−2, see ESI† for the GCD measurements and corresponding calculations, Fig. S12†). Still, the current densities and discharging capacities of MoO3 reported for similar potential ranges and discharging times (∼10 mA cm−2 and ∼100 μA h cm−2, respectively)7,62 are ten-fold higher. The difference is explained by the electrodes' specific structuring rather than the reported materials' superior behavior.7,62 If the entire surface of the PAA-free OX48-180 sample were involved in the analysis, it would exhibit enhanced characteristics and be highly competitive for the desired application.
Further, Dunn's approach7,64 was adopted to deconvolute CV current into diffusive and capacitive current contributions:
i(V, ν) = k1(V)ν + k2(V)ν1/2 | (3) |
i(V, ν)/ν1/2 = k1(V)ν1/2 + k2(V) | (4) |
Charging:
MoVIO3 + Na+ + e− → NaMoVO3 | (5) |
MoV2O5 + Na+ + e− → NaMoIVMoVO5 | (6) |
Discharging:
NaMoVO3 → MoVIO3 + Na+ + e− | (7) |
NaMoIVMoVO5 → MoV2O5 + Na+ + e− | (8) |
This CV deconvolution analysis eventually confirms that the A1, A2, and C1 peaks are due to the capacitive, diffusive, and mixed contributions, respectively.
An extra contribution to the diffusive current at potentials below −1.8 V vs. Ag/AgCl (Fig. 11e) is attributed to the hydrogen evolution reaction. It occurs at less negative potentials than initially assumed (i.e., beyond −2.0 V vs. Ag/AgCl; see Fig. S10†). The extra ‘peak’ in the capacitive current at −0.3 V vs. Ag/AgCl (Fig. 9d) is likely an artifact of the deconvolution since this approach does not consider the peak shift effect with increasing sweep rate.64 Finally, the ratios of capacitive and diffusive contributions to the CV curves are calculated for each scan rate (Fig. 11f). The capacitive current dominates at the higher scan rates, while the diffusive contribution is more significant at the lower scan rates.
The scan-rate-dependent CVs (Fig. 11a) are used to calculate the specific charging and discharging capacities and to estimate the rate capability of the OX48-180 film (Fig. 11g). The difference between the charging and discharging capacities, especially at the low scan rates, is attributed to a substantial negative current due to the hydrogen evolution during the cathodic and anodic sweeps, which lowers the efficiency of the electrode in the investigated potential window. Therefore, a narrower window is needed for practical use, limited by −1.6 V vs. Ag/AgCl. An insignificant decrease in discharging capacity from ∼4 to 3 μA h cm−2 with increasing scan rate implies an excellent rate capability of the electrode.7,67
Future work is required to thin the shells and increase their electron conductivity. This might be achieved by playing with anodization variables, applying post-anodizing surface-finishing techniques such as partial wet or plasma chemical fine polishing, doping the shells with electron-conducting elements or compounds, or nitridation techniques.74 Alternatively, the as-prepared nanoarrays seem highly appropriate without additional treatments as building blocks for nanostructured field-emission, memristive, superconducting, magnetic, or optical nanodevices – where the heterogeneous core/shell nanostructure may be highly advantageous.13,58,74 These will be the subjects of future research.
(1) For the first time, arrays of MoOx-based nanostructures of various sizes and morphologies, vertically aligned on a substrate, have been synthesized self-organized via the PAA-assisted anodization of a Mo layer through a very thin Nb interlayer. Such a smart anodization enabled the nucleation and sustainable growth of fully amorphous MoOx nanostructures within and under the PAA nanopores, which is impossible by direct molybdenum anodizing or other methods.
(2) The oxide growth occurred via the unique outward migration of Mon+ and Nb5+ ions through the thin Nb2O5 interlayer, alumina barrier layer, along the pore walls, and inside the pores together with the inward migration of O2− (OH−) ions. Such a cooperative ion transport resulted in a self-organized core/shell architecture of the oxide protrusions: the shells comprise MoO3, molybdenum suboxides (Mo5+ and Mo4+), Nb2O5, and Al2O3 mixed at the molecular level, whereas the cores are partially hydrated and slightly reduced pure MoO3. The 550 °C annealing in ambient air or a vacuum (10−5 Pa) results in an amorphous-to-crystalline transition in the bottom-oxide layers and partial oxidation of the suboxides in the shells.
(3) The cores of the oxide nanorods exhibit electron transport properties of a highly-doped n-type semiconductor, with Nd reaching 1 × 1022 cm−3, while the shells are less doped semiconductors or dielectrics.
(4) The MoOx-based nanoarrays revealed the potential for applications in semiconductor nanoelectronics where the intensive and localized at the nanoscale electron transport, reversible redox reactions, high population density of nanochannels (up to 3 × 1010 cm−2), and tailored crystallinity are in demand. The disclosed intercalation pseudocapacitance behavior of the rods' cores and the competitive performance metrics make the films promising as nanostructured electrodes for on-chip energy-related applications. The works to improve the electron-transport properties of the shells, explore field-emission and memristive potentials of the nanoarrays, and design relevant device configurations are in progress and will be reported in due course.
Footnote |
† Electronic supplementary information (ESI) available: Anodizing curves, SEM images, XPS- and XRD-related data, calculations, additional electrochemical data. See DOI: https://doi.org/10.1039/d5ta02921j |