The industrial synthesis of functional polyolefins relies on free radical polymerization, which requires high temperature and pressure and offers poor microstructure control. Herein, we report a cation-switching strategy to access ethylene and alkyl acrylate copolymers with made-to-order molecular weight, molecular weight distribution, and polar monomer density, tunable within a catalyst-dependent range. This precision was achieved by exploiting the cation exchange dynamics between M+ and M′+ (where M+, M′+ = Li+, Na+, K+, or Cs+, and M ≠ M′) with our nickel phenoxyphosphine-polyethylene glycol catalyst. Under non-switching conditions, copolymerization of ethylene and methyl acrylate (MA) using our nickel catalyst in the presence of M+ and M′+ salts afforded ethylene-MA copolymers (EMA) with adjustable molecular weight distributions based on the ratio of M+
:
M′+ employed. Under dynamic cation switching conditions, this catalyst system yielded monomodal EMA with molecular weight and MA incorporation that can be varied independently. Studies of the EMA revealed that while they retain the thermal and mechanical properties of polyethylene having the same molecular weight, increasing the MA per chain by as few as 1–3 units leads to measurable increase in their wettability and susceptibility toward oxidative cleavage. This work adds to a growing body of evidence suggesting that ethylene-based materials can be designed for improved degradability without compromising their performance.
Another approach to prepare EAA is through the coordination–insertion copolymerization of ethylene and alkyl acrylate using transition metal catalysts (Chart 1B, option II).11–17 This method can provide EAA with narrow dispersity (Đ < 2), variable polar monomer content, and even ultra-high molecular weight (Mn > 103 kg mol−1).18 However, obtaining EAA with user-defined specifications remains a significant challenge. For example, increasing the alkyl acrylate concentration in the copolymerization reaction can enhance the polar content in the resulting polymer but the molecular weight typically decreases and vice versa.19–22 Thus, independently varying a single parameter in copolymerization, such as MW, MW distribution (MWD), or polar group incorporation, without impacting another is difficult to achieve.
To overcome the limitations of a one catalyst-one polymer paradigm,23 our group has focused on the development of cation-tunable polymerization catalysts.24–26 Unlike other strategies that rely on light,27 redox agents,28–31 or boranes,32,33 the use of secondary metal cations with polymerization catalysts offers the potential to access more than two reactivity states.34 For example, metal cations can differ in charge, Lewis acidity, and size, which can modulate a catalyst's steric and electronic properties to different extent. A variety of Ni/Pd catalyst platforms have been demonstrated to be cation-tunable, including those based on P,O-,25,26,35–37N,O-,24,38 and C,O-donors.39 Our recent discovery that cation exchange equilibria could be manipulated to influence the coordination–insertion of non-living polymerization catalysts affords another level of control.40 Under non-switching conditions, the polymerization of ethylene using our nickel phenoxyphosphine polyethylene glycol (PEG) catalysts with M+ and M′+ (where M+, M′+ = Li+, Na+, K+, or Cs+; and M+ ≠ M′+) yielded bimodal PE with adjustable MWD depending on the M+
:
M′+ ratio employed. In contrast, under dynamic cation switching conditions, the same catalyst system generated monomodal PE with tunable MW as a function of the M+
:
M′+ ratio. However, these studies were performed in the presence of only ethylene so it was unclear whether polar monomers would be compatible with this polymerization strategy.
In this work, we successfully expanded the application of dynamic cation switching to ethylene and alkyl acrylate copolymerization, enabling for the production of functional polyolefins with high precision (Chart 1B, option III). We demonstrate that ethylene-methyl acrylate copolymers (EMA) can be made-to-order with specific MW, MWD, and polar group incorporation, tunable within a catalyst-dependent range. Having access to a series of systematically varied EMA allowed us to interrogate their structure–function relationships, offering new insights into the properties of this important class of polymers.
Although we have shown that the cation exchange rates between our Ni complexes and M+ can be controlled by solvent polarity (i.e., polar mixtures facilitate fast exchange whereas non-polar mixtures facilitate slow exchange),40 we were unsure whether polar monomers would affect these rates. To interrogate this possibility, we conducted a series of cation binding studies. In these experiments, Ni1 was dissolved in toluene-d8/Et2O (48
:
2) and then various amounts of NaBArF4 were added. The mixtures were stirred for 10 min and then analyzed by 31P NMR spectroscopy. The starting Ni1 complex showed two doublets centered at −12.1 and 13.4 ppm (J = 319 Hz), consistent with having a trans arrangement of the two phosphine donors around the nickel square plane (Fig. 1A, trans-Ni1).41,42 The cis-Ni1 isomer, in which the phosphine ligands are adjacent to each other in the nickel center, was not observed. In the absence of methyl acrylate (MA), the addition of up to 1.0 equiv. of Na+ resulted in the appearance of two sets of signals (Fig. 1B). The first set of peaks shifted upfield as increasing quantities of Na+ were added, ultimately centering at −15.9 and 10.3 ppm (J = 319 Hz). We propose that these peaks arise from signaling average of trans-Ni1 and trans-Ni1–Na species interconverting on the NMR timescale, suggesting that cation exchange occurs readily in this solvent mixture. The second set of signals at −8.4 and 10.8 ppm grew in intensity but did not shift when greater amounts of Na+ were introduced. These resonances were assigned to the two phosphines in cis-Ni1–Na based on their J coupling constant of 34 Hz.42 Because the starting nickel species does not exist in the cis form, there is no possibility of cis-Ni1 and cis-Ni1–Na equilibration.
Next, the binding of Na+ to Ni1 was evaluated in the presence of 0.05 M methyl acrylate in toluene-d8/Et2O (48
:
2) (Fig. 1C). We observed that the 31P NMR spectra of the Ni1 and Na+ samples with and without MA additives were nearly identical, indicating that the presence of polar monomers at the concentration tested had minimal effects on the cation binding dynamics. Additional experiments conducted using Ni1 and CsBArF4 in toluene-d8/Et2O (48
:
2) showed similar behavior (Fig. S3). Specifically, the treatment of Ni1 with Cs+ led to the formation of heterobimetallic trans-Ni1–Cs and cis-Ni1–Cs species. Once again, signal averaging between the trans-Ni1 and trans-Ni1–Cs peaks suggests that cation exchange is fast in this solvent mixture. However, under catalytic conditions, the MA
:
catalyst stoichiometry is typically 1250
:
1 rather than 1
:
1 so we expect that MA will have a more significant impact on the cation binding behavior in polymerization (vide infra). Although it might be possible to use other polar co-solvents such as tetrahydrofuran or dioxane, we prefer diethyl ether because it is less coordinating, minimizing possible catalyst inhibition effects.
:
2) under ethylene at 30 °C (Fig. 2; Table S1, entry 3). After 0.5 h, the reaction was quenched with acid and the resulting white solid was characterized by 1H NMR spectroscopy. The broad peaks at ∼2.5 and 3.7 ppm were assigned to in-chain methyl ester groups,17,45,47 confirming that the desired EMA was obtained (Fig. S39). Further characterization of the copolymer showed that it has an average molar mass (Mn) of 2.2 kg mol−1 with 1.08 mol% incorporation of MA and dispersity (Đ) of 1.1. We found that decreasing the Ni1 catalyst loading to 0.5 µmol (Table S1) or increasing the MA concentration to 0.25 M (12.5 mmol, Table S2) resulted in no product. Because MA can inhibit the nickel catalyst via coordination by its oxygen donor rather than C
C bond, increasing the MA
:
catalyst ratio often leads to lower catalyst activity.19,21,48 Finally, extending the polymerization time from 0.5 to 2.0 h led to a reduction in catalyst activity from 328 to 227 kg mol−1 h−1 (Table S3), presumably due to catalyst decomposition.49
To study the effects of cations on Ni1, we performed ethylene and MA copolymerization studies in the presence of various alkali ions using our optimized conditions at 30 °C (Table 1). The use of MBArF4 is preferred over other MX salts (where X− = BPh4−, SO3CF3−, etc.) because the BArF4− anion acts as a non-coordinating spectator ion.41 Our data revealed that catalyst activity decreased from 1020 to 196 kg mol−1 h−1 whereas the MA incorporation increased from 0.71 to 1.26 mol% mostly according to the order Li+ → Na+ → K+ → Cs+ (entries 2–5). In contrast, the polymer MW did not follow an obvious trend, with Ni1–Li (Mn = 18.9 kg mol−1) and Ni1–Na (Mn = 2.2 kg mol−1) giving the highest and lowest, respectively. As a control, reactions in the absence of M+ gave no products (entry 1). These results are qualitatively similar to those observed previously with Ni1–M in ethylene homopolymerization,26,41 except that the catalyst activities and polymer MWs are lower in the present study due to the inhibiting effects of MA. Based on independent computational investigations of this nickel system by Ratanasak, Parasuk, and coworkers,50 it was proposed that the energy barriers associated with the elementary steps in coordination–insertion of ethylene (e.g., cis–trans nickel isomerization, olefin insertion, and olefin binding) are lowest in the presence of Li+ and highest in the presence of Cs+. Their density functional theory (DFT) results are consistent with our experimental observations that the catalyst activity follows the periodic trend from Li+ → Na+ → K+ → Cs+. Our results showing that the more active Ni1–M catalysts yielded copolymers with lower MA mol% indicate that ethylene insertion is faster relative to MA insertion. However, further mechanistic studies of the copolymerization process are necessary to identify the rate-determining steps and evaluate whether there are cooperative interactions between MA and the metal centers in Ni1–M.51,52 The Ni1–M catalysts were also capable of producing ethylene-ethyl acrylate (EEA) and ethylene-tert-butyl acrylate (EBA) copolymers from ethylene and the corresponding comonomer (Table 1, entries 6–10).
| Entry | M+ | Acrylate | Act. (kg mol−1 h−1) | Inc.b (mol%) |
M
n c (kg mol−1) |
Đ | Acrylate/chaind | T m (°C) |
|---|---|---|---|---|---|---|---|---|
| a Polymerization conditions: Ni1 catalyst (2 µmol), MBArF4 (4 µmol), Ni(COD)2 (8 µmol), ethylene (400 psi), alkyl acrylate (2.5 mmol, 0.05 M), 48 mL toluene/2 mL Et2O, 30 °C, 30 min. In the absence of cations, Ni1 is not active for polymerization. Temperature was controlled by manual external cooling when necessary to ensure that the reaction temperature did not exceed 5 °C from the starting temperature. b Determined by 1H NMR spectroscopy. See SI for the equations used. The standard deviations are typically less than 7%. c Determined by GPC in trichlorobenzene at 160 °C. The standard deviations are typically less than 10%. Abbreviations: MA = methyl acrylate, EA = ethyl acrylate, BA = tert-butyl acrylate. d See SI for calculations. | ||||||||
| 1 | None | MA | 0 | — | — | — | — | — |
| 2 | Li+ | MA | 1020 | 0.71 | 18.9 | 1.4 | 4.7 | 125 |
| 3 | Na+ | MA | 328 | 1.08 | 2.2 | 1.1 | 0.8 | 107 |
| 4 | K+ | MA | 340 | 1.12 | 3.1 | 1.4 | 1.2 | 115 |
| 5 | Cs+ | MA | 196 | 1.26 | 12.3 | 1.6 | 5.4 | 119 |
| 6 | Li+ | BA | 843 | 0.26 | 14.8 | 1.3 | 1.4 | 124 |
| 7 | Na+ | BA | 492 | 0.58 | 2.3 | 1.4 | 0.5 | 112 |
| 8 | K+ | BA | 467 | 0.76 | 3.7 | 1.8 | 1.0 | 121 |
| 9 | Cs+ | BA | 312 | 0.89 | 15.1 | 1.5 | 4.7 | 116 |
| 10 | Li+ | EA | 366 | 0.2 | 11.7 | 1.5 | 0.8 | 124 |
Because Ni1–Cs appeared to show greater thermal stability than the other Ni1–M catalysts, we also evaluated its activity at different temperatures (Fig. 2 and Table S4). Our results indicated that Ni1–Cs has maximum activity at 70 °C (512 kg mol−1 h−1) but still gave EMA with appreciable rates at 90 °C (485 kg mol−1 h−1). At 70 °C, the activity of Ni1–Cs was noticeably higher than at 30 °C, with up to 988 kg mol−1 h−1 for the copolymerization of ethylene and tert-butyl acrylate (Table S6).
Compared to other metal catalysts that have been reported for ethylene and alkyl acrylate copolymerization, the Ni1–M complexes are among the top-performers (Fig. 3; see Table S20 for more examples).53,54 The most active nickel catalysts are all based on the phenoxyphosphine ligand platform.22,43–45 This catalyst family includes Ni3 with 2,6-diisopropyloxyphenyl phosphine substituents18 and Ni4 that is immobilized on magnesium oxide support.55 For comparison purposes we will use Ni1–Li as a representative example of our cation-tunable catalysts. Based on the copolymerization data, the rankings are as follows: Ni3 > Ni1–Li > Ni4/MgO for activity and Ni3 > Ni4/MgO > Ni1–Li for polymer molecular weight. All three nickel catalysts gave EMA with <1.0 mol% of MA incorporation. One of the most active palladium catalysts reported for ethylene and MA copolymerization is Pd1,56 which features a phosphine-phosphine oxide ligand. This palladium catalyst compares favorably with the nickel catalysts but it provided EMA with a molecular weight of only 7 kg mol−1.
![]() | ||
| Fig. 3 Representative examples of the most active catalysts for ethylene and methyl acrylate copolymerization reported to date. See Fig. S28 and Table S20 for more examples. | ||
:
M′+ ratio used in the reaction.
In slightly polar solvents, we anticipate that combining our nickel catalyst with M+ and M′+ would generate active nickel species that continuously cycle between Ni/M+ and Ni/M′+ states during chain propagation (i.e., if cation switching is faster than the termination) (Scheme 1B). For example, starting from species I, exchange of M+ with M′+ will afford Ni(P)–M′ (V), which is capable of promoting further ethylene and MA insertions to VI. This propagating species can undergo cation exchange to VII as the reaction continues. Because each polymer chain is derived from a single active species that switches between two states, adjusting the M+
:
M′+ ratio determines the extent in which Ni/M+ and Ni/M′+ controls the growth of individual polymer chains. This strategy would enable precise fine-tuning of the polymer microstructure, achieving a level of control beyond what is feasible through reaction engineering.
To determine if cation switching can occur in the presence of polar monomers, we performed ethylene and MA copolymerizations in different solvent mixtures (Fig. 4). When Ni1 was combined with CsBArF4/NaBArF4 (1
:
1 ratio, 1 equiv. each relative to Ni), Ni(COD)2, ethylene, and MA under standard conditions, we obtained EMA with different MWD depending on the polarity of the solvent used. The gel permeation chromatograms (GPC) showed that the EMA obtained from reactions in 49.8
:
0.2 and 48
:
2 toluene/Et2O mixtures were bimodal whereas those obtained from reactions in 47
:
3 and 46
:
4 toluene/Et2O mixtures were monomodal or nearly so (Đ < 2.0; Fig. 4, bottom left). These results suggest that in less polar solvents, cation exchange between Ni1–Cs and Ni1–Na is slow so polymer chain growth occurs from two distinct active species. As the solvent polarity is increased, each nickel catalyst switches continuously between two different states (Ni1/Cs+ and Ni1/Na+) during chain propagation so only a single polymer population is produced. When this study was conducted using Ni1 with LiBArF4/NaBArF4, similar results were obtained except that monomodal EMA was observed in the 48
:
2 toluene/Et2O mixture (Fig. 4, bottom right). Because the minimum solvent polarity needed to achieve dynamic cation switching is dependent on the binding affinity of the specific cations to Ni1, different salt combinations will require different toluene/Et2O mixtures. Increasing the amount of Et2O used in the reactions decreased the catalyst activity, most likely due to the solvent serving as a competing ligand for the nickel active sites (Tables S7 and S8).
:
Na+ ratio while keeping the Ni1, Ni(COD)2, ethylene, and MA amounts constant in a 49.8
:
0.2 mixture of toluene/Et2O (Fig. 5 and Table S9). Analysis of the resulting EMA revealed that in all cases, bimodal polymers were obtained, in which their MWD is skewed toward the higher molecular weight end if the ratio of Li+
:
Na+ was higher and vice versa. Deconvolution of the GPC traces obtained from the 3
:
1 Li+
:
Na+ reaction showed a higher molecular weight peak A and a lower molecular weight peak B with an integrated ratio A/B of 0.86. When the Li+
:
Na+ ratio was changed to 1
:
1 and 1
:
3, the A/B values dropped to 0.27 and <0.26, respectively. We were unable to fit the minor component (peak A) in the 1
:
3 Li+
:
Na+ data to a Gaussian distribution so the A/B value calculated is likely an upper limit. These results are consistent with our proposed mechanistic model (Scheme 1A) because using more Li+ relative to Na+ salt favors the formation of higher MW producing Ni1–Li over the lower MW producing Ni1–Na (Table 1).
To achieve option 1, we used Li+ and Na+ salts with Ni1 because the corresponding Ni1–Li and Ni1–Na species afford EMA with different molecular weight and MA incorporation (Table 2, entries 2–6). The copolymerizations were performed in 48
:
2 toluene
:
Et2O to promote fast cation exchange. When greater amounts of Li+ were added relative to Na+, the EMA molecular weight increased gradually from ∼6 to 18 kg mol−1 whereas the MA incorporation decreased gradually from ∼1.1 to 0.7 mol% (Fig. 6A). The monomodal distributions (Fig. S11) and polymer dispersity of <2.0 strongly suggest that the products were generated by a single active species, which supports a dynamic cation switching mechanism (Scheme 1B). To achieve option 2, we paired Ni1 with Cs+ and Na+ salts (toluene/Et2O = 47
:
3) because the Ni1–Cs and Ni1–Na species formed will produce EMA with different MW but similar MA incorporation (Table 2, entries 9–13). Our data showed that increasing the Cs+
:
Na+ ratio increased the EMA molecular weight from ∼3 to 8 kg mol−1 while keeping the MA incorporation within a narrow range (Δincorp. = 0.2 mol% going from 1
:
3 to 5
:
1 Cs+
:
Na+) (Fig. 6B). Finally, to achieve option 3, a combination of Li+ and Cs+ cations were used with Ni1 (toluene/Et2O = 47
:
3) because the resulting Ni1–Li and Ni1–Cs generated will yield EMA with similar MW but different MA incorporation. As shown in Fig. 6C, increasing Li+ relative to Cs+ generated copolymers featuring an average Mn of ∼19 kg mol−1 but decreasing MA incorporation from 1.4 to 1.0 mol% (Table 2, entries 16–20).
![]() | ||
| Fig. 6 Plots showing the use of Li+/Na+ (A), Cs+/Na+ (B), or Li+/Cs+ (C) with Ni1 under dynamic cation switching conditions to obtain EMA with varying molecular weight and MA incorporation. For comparison, EMA synthesis was attempted by varying the MA concentration using Ni1–Cs (D). The empirical formulas for each polymerization set were derived from mathematical fitting. The polymerization data are provided in Tables 2 and S10–S12. | ||
| Entrya | M+ : M′+ ratio |
Act. (kg mol−1 h−1) | Inc.b (mol%) |
M
n c (kg mol−1) |
Đ | MA/chaind |
T
m e (°C) |
|
|---|---|---|---|---|---|---|---|---|
a The toluene : Et2O ratio was 48 : 2 for Li+/Na+ and 47 : 3 for Cs+/Na+ and Li+/Cs+.
b Determined by 1H NMR spectroscopy. The standard deviations are typically less than 7%.
c Determined by GPC in trichlorobenzene at 160 °C. The standard deviations are typically less than 10%.
d See SI for equations used.
e Measured using DSC.
|
||||||||
| 1 | Li+ : Na+ |
2 : 0 |
1020 | 0.71 | 18.9 | 1.4 | 4.7 | 125 |
| 2 | Li+ : Na+ |
5 : 1 |
913 | 0.73 | 18.5 | 1.3 | 4.7 | 123 |
| 3 | Li+ : Na+ |
3 : 1 |
686 | 0.83 | 15.4 | 1.6 | 4.5 | 124 |
| 4 | Li+ : Na+ |
2 : 1 |
690 | 0.96 | 15.9 | 1.4 | 5.0 | 123 |
| 5 | Li+ : Na+ |
1 : 1 |
597 | 1.04 | 11.8 | 1.2 | 4.3 | 123 |
| 6 | Li+ : Na+ |
1 : 3 |
397 | 1.11 | 6.0 | 1.3 | 2.3 | 114 |
| 7 | Li+ : Na+ |
0 : 2 |
328 | 1.08 | 2.2 | 1.1 | 0.8 | 107 |
| 8 | Cs+ : Na+ |
2 : 0 |
102 | 1.45 | 17.8 | 1.3 | 8.9 | 117 |
| 9 | Cs+ : Na+ |
5 : 1 |
147 | 1.50 | 8.3 | 1.3 | 4.3 | 115 |
| 10 | Cs+ : Na+ |
3 : 1 |
154 | 1.43 | 6.6 | 1.7 | 3.2 | 117 |
| 11 | Cs+ : Na+ |
2 : 1 |
162 | 1.35 | 5.9 | 1.2 | 2.8 | 116 |
| 12 | Cs+ : Na+ |
1 : 1 |
144 | 1.34 | 4.6 | 1.4 | 2.1 | 113 |
| 13 | Cs+ : Na+ |
1 : 3 |
262 | 1.31 | 3.4 | 1.5 | 1.5 | 111 |
| 14 | Cs+ : Na+ |
0 : 2 |
266 | 1.15 | 3.1 | 2.3 | 1.2 | 107 |
| 15 | Li+ : Cs+ |
2 : 0 |
664 | 0.92 | 16.9 | 1.6 | 5.4 | 122 |
| 16 | Li+ : Cs+ |
5 : 1 |
636 | 1.03 | 18.4 | 1.3 | 6.6 | 123 |
| 17 | Li+ : Cs+ |
3 : 1 |
529 | 1.08 | 19.6 | 1.5 | 7.4 | 123 |
| 18 | Li+ : Cs+ |
2 : 1 |
522 | 1.14 | 19.1 | 1.3 | 7.6 | 120 |
| 19 | Li+ : Cs+ |
1 : 1 |
510 | 1.21 | 19.7 | 1.6 | 8.2 | 118 |
| 20 | Li+ : Cs+ |
1 : 3 |
161 | 1.41 | 20.6 | 1.6 | 10.1 | 118 |
| 21 | Li+ : Cs+ |
0 : 2 |
102 | 1.45 | 17.8 | 1.3 | 8.9 | 117 |
The data above were fit to mathematical functions, providing empirically derived formulas for calculating the amount of M+ and M′+ salts needed to obtain copolymers with a specific set of characteristics (Fig. 6A–C).40 Equations correlating “z” (Mn) with “x” (M+/M′+ molar fraction) and “y” (MA incorporation) with “x” were determined for each Ni1/M+/M′+ combination. Three-dimensional exponential and/or polynomial equations can be used to relate all 3 variables (x, y, and z) and are given in the SI (Fig. S16, S19, and S22). Although theoretical modeling of the experimental data may be possible, it would be difficult given that the rates of various elementary steps and cation association/dissociation processes are needed to fully describe the polymerization process. These empirical relationships are useful because they allow prediction of the polymer products attainable using any combination of Ni1/M+/M′+ that has been tested (Table S13).
To compare the effectiveness of our strategy vs. that of a typical approach to customize EMA, we carried out ethylene and MA copolymerization using Ni1–Cs under standard conditions but with varying concentrations of the polar monomer (Fig. 6D and Table S14). We observed that increasing the MA concentration from 0.01 to 0.10 M afforded EMA with decreasing molecular weight (21 to 6 kg mol−1) but increasing MA incorporation (0.42 to 1.77 mol%). The inverse relationship between polymer MW and MA incorporation is expected because the presence of acrylates can induces faster chain termination.44 At higher MA concentration, the Ni1–Cs activity dropped significantly, from 532 to 46 kg mol−1 h−1. When 0.25 M methyl acrylate was used, the catalyst was completely inactive. These results are consistent with previous studies showing that polar monomers can inhibit polymerization through engaging in σ interactions with the metal catalyst.63 Because our strategy does not require changing the MA concentration to adjust the polymer composition, moderate to high activities (>100 kg mol−1 h−1) were obtained in our copolymerizations (Table 2).
To determine the microstructures of the copolymers, we relied on characterization using 1H and 13C NMR spectroscopy. We observed that in most cases, the MA units in EMA are located primarily in-chain,43,64,65 as revealed by the 1H NMR signal at 3.71 ppm and the 13C NMR signal at 176 ppm corresponding to the methyl and carbonyl groups of MA, respectively (Fig. S39–S49). Similarly, the ethylene/tert-butyl acrylate copolymers were found to also contain in-chain BA groups (Fig. S56 and S57). The exception to this trend is copolymers synthesized using more polar solvent mixtures (e.g., 45
:
5 toluene
:
Et2O, Fig. S65–S68), which featured both in-chain and chain-end polar moieties. Given that under our standard polymerization conditions we obtained copolymers with mostly in-chain polar groups, insertion of alkyl acrylate into the Ni-polymeryl species does not appear to induce chain termination.44
Although the “tunable range” in these experiments is somewhat narrow (e.g., Mn between ∼3 to 8 kg mol−1 using Cs+/Na+ and MA incorporation between 1.0 to 1.4 mol% using Li+/Cs+), this restriction is due to limitations of the Ni1 catalyst rather than the tuning method. We expect that Ni2 (Scheme S1),40 which can give polyethylene with Mn of >1000 kg mol−1 in the presence of Cs+, will likely afford access to EMA with a wider range of molecular weights.
Next, we investigated the physical properties of the copolymers as a function of MA. All measurements were performed on polymers with an average molecular weight of ∼20 kg mol−1 and average MA incorporation of 0 (PE-1), 0.8 (EMA-1), 1.1 (EMA-2), and 1.4 mol% (EMA-3) (Table 3). The polymer specimens were molded into a T-bone shape and then subjected to tensile testing. The stress vs. strain curves (Fig. S24 and S25) showed that all of the materials evaluated have similar mechanical properties, with elongation at break ranging from 8–10% and tensile strength between 19–23 MPa (Table 3). These values are typical for high-density polyethylene, which can range from 3–1900% and 3–60 MPa for elongation-at-break and tensile strength, respectively.68 Our results suggest that the presence of small amounts of MA in the polymer chain has negligible impact on its mechanical properties.
| Polymer | Inc. (%) | MA per chain | M n (kg mol−1) | Elong. at break (%) | Tensile strength (MPa) | Contact angle (°) | PI |
|---|---|---|---|---|---|---|---|
| a Values shown are the average from two independently prepared samples with similar MA incorporation and Mn. The maximum standard deviations is ±0.1 mol% for MA incorporation and ±2 kg mol−1 for MW. See Table S18 for more details. PI = peroxide index. | |||||||
| PE-1 | 0 | 0 | 19 | 9.2 | 19.7 | 107.8 | 5 |
| EMA-1 | 0.8 | 6.6 | 23 | 10.4 | 23.2 | 99.6 | 7.9 |
| EMA-2 | 1.1 | 7.8 | 20 | 10.5 | 21.2 | 97.8 | 7.6 |
| EMA-3 | 1.4 | 10.5 | 21 | 8.4 | 20.1 | 94.0 | 16.4 |
To determine the wettability of the polymer samples, their water contact angles were measured using a static drop method at 25 °C (Fig. S26).69,70 We found that PE-1 had an average contact angle of 107.8°, which is within the range expected for polyethylene.71,72 When the methyl acrylate content increased to 7 (EMA-1), 8 (EMA-2), and 10 (EMA-3) units per chain, the water contact angle decreased to 99.6, 97.8, and 94.0°, respectively (Table 3), indicating that the EMA-coated surface became increasingly more polar.4,73–75
Inspired by reports on the reactions of peroxides with polyethylene,85–87 we focused on developing polymer degradation methods that can be performed under mild oxidizing conditions. We found that stirring PE-1, EMA-1, EMA-2, or EMA-3 in the presence of tert-butylperoxy-2-ethylhexyl carbonate (TBEC) in H2O at 75 °C for 24 h was sufficient to promote polymer degradation (Fig. 7A). The solid products were isolated by filtration, washed with water and acetone, and then dried overnight. The recovered mass was up to ∼90% of the starting mass (Table S17), suggesting that the material isolated represents the bulk of the TBEC-treated products. To determine the extent of degradation, we analyzed the products by GPC and calculated the reduction in molecular weight percentage (ΔMn) using the formula: (MWi − MWf)/MWi × 100%, in which MWi is the initial molecular weight and MWf is the final molecular weight (Table S17). In the absence of peroxide, the ΔMn did not exceed ∼15% regardless of whether the polymer contained MA (Fig. 7A). In contrast, the addition of TBEC to the reactions led to significant changes in polymer molecular weight. For example, PE-1 had an average ΔMn value of 74% and EMA-1, EMA-2, and EMA-3 had average ΔMn values of 88, 92, and 97%, respectively. The peroxide indices (PI), defined as ΔMn in the presence of peroxide divided by ΔMn in the absence of peroxide, were 5.0, 7.9, 7.6, and 12.9, respectively (Table 3). These results indicated that: (1) appreciable polymer degradation occurred only under oxidative conditions and (2) the polymer degradation efficiency was enhanced upon introducing more MA per chain, requiring only 1–3 units to achieve measurable effects.
To determine whether the presence of EMA can enhance the degradability of PE, we combined both polymers (1
:
1 mixture of PE and EMA containing 1.0 mol% MA; average Mn = 18.7 kg mol−1) in H2O with TBEC and stirred the sample for 24 h at 75 °C (Table S17). Our results showed that the average ΔMn was about 82%, which is higher than that for PE (74%) but lower than that for EMA containing 1.0 mol% MA (∼90%) (Fig. S101). Interestingly, this ΔMn value is expected for EMA containing 0.5 mol% polar density. Thus, these results indicate that the degradation efficiency can be predicted based on the total MA composition in a polymer mixture, regardless of whether the polar groups are located on the same chain.
The TBEC-treated polymers were further characterized to determine their composition. 1H NMR spectroscopic analysis of the degraded PE-1 product showed a new peak at ∼2.4 ppm that was assigned to α-keto hydrogens (∼0.75 mol%; Fig. 7B and S83).65 The 1H NMR spectrum of degraded EMA-2 exhibited new peaks at 2.4 and 9.8 ppm, which were attributed to α-keto (∼1.0 mol%) and aldehyde (<0.1 mol%) hydrogens, respectively (Fig. 7B and S85). The MA content in degraded EMA-2 dropped from ∼1.1 to 0.5 mol%. Signals corresponding to C–H hydrogens from alcohol moieties (∼3.6 ppm) were not detected in any of the samples. Attempts to observe the C
O peaks in the 13C NMR spectra were unsuccessful (Fig. S100), most likely due to the low concentration of carbonyl groups in the polymer samples and their inherently weak NMR signals.
To support the NMR spectral assignments, we also measured the infrared (IR) spectra of the degraded polymers. Comparison of the vibrational data for PE-1 before and after treatment with TBEC, revealed a new peak at 1715 cm−1 that corresponds to the C
O stretch of ketone groups (Fig. 7C, left). The IR spectrum of degraded EMA-2 also exhibited a ketone peak at 1715 cm−1, along with an ester peak at 1740 cm−1, suggesting that some of the methyl ester groups were intact (Fig. 7C, right).88 The presence of O–H stretches between ∼2500–3500 cm−1 corresponding to alcohol or carboxylic acid moieties were not detected.
Based on other studies of polymer degradation, the products observed suggest that TBEC-induced chain scission likely proceeded through a radical oxidation mechanism (Scheme S4).89,90 Such sequences are typically initiated by H-atom abstraction by a reactive oxygen species,85 followed by propagation involving oxygenation and homolytic O–O or C–C bond scission. Given the absence of molecular weight increase and gelation in our samples, cross-linking through radical chain recombination did not appear to occur. Unlike work reported by Nozaki and coworkers on the use of dioxygen, a cerium catalyst, and visible light to degrade carboxylated polyethylene, which generated products with ketone, aldehyde, alcohol, and carboxylic acid groups,65 our TBEC-based method afforded products with only ketone and minor amounts of aldehyde in EMA. We hypothesize that the enhanced degradability of EMA relative to that of PE is due to the weakening of the C–H and C–C bonds in close proximity to the polar group, which makes undergoing radical reactions more facile. The high mass recovery in our degradation studies suggests that overoxidation to CO2 is suppressed. To add value to the degraded PE and EMA products, it may be possible to convert them to paraffin waxes (C20–C30)91 or cross-link them with reversible linkers (e.g., by using α,ω-diaminoalkane to condense with the carbonyl groups in the degraded polymers) to construct chemically-recyclable materials.92,93 Additionally, the ketone groups can be converted to esters through Baeyer–Villiger oxidation94–96 or treated with hydroxylamine to form amides via Beckmann rearrangement.96,97
:
0.2 toluene/Et2O gave bimodal EMA whereas 47
:
3 toluene/Et2O gave monomodal EMA) and M+
:
M′+ ratio. To demonstrate the utility of our method, we successfully prepared three sets of copolymers: (1) EMA with different MW and MA incorporation; (2) EMA with different MW but similar MA incorporation; and (3) EMA with different MA incorporation but similar MW. When we attempted to tune the polar group density by increasing the MA concentration, the resulting copolymers had higher MA incorporation but reduced MW. Using larger amounts of MA had detrimental effects on the catalyst activity because MA can inhibit the catalyst via σ-coordination. These results suggest that dynamic cation switching polymerization affords a much higher level of control over the polymerization outcome compared to other approaches that rely on reaction optimization or engineering, which can be particularly useful in situations where the reaction conditions needed are impractical to achieve (e.g., in industrial reactors that are designed to operate within certain temperatures or pressures). Free radical and coordination–insertion polymerization are complementary methods, as the former enables the synthesis of copolymers with high polar group content (e.g., >50 mol%) whereas the latter is better suited for generating copolymers with lower polar group content (e.g., <5 mol%).
Although low-polarity polyethylene has not traditionally been regarded as a valuable material, our research indicates that they exhibit unique and useful properties worthy of further investigations. For example, studies of PE-1, EMA-1, EMA-2, and EMA-3 demonstrated that the copolymers had similar thermal and mechanical properties as those in the ethylene homopolymer but exhibit greater wettability, which could enhance their adhesiveness and compatibility with other materials. Our finding that only minor quantities of MA per chain are sufficient to increase their susceptibility toward oxidative chain scission is significant, suggesting that polymers could be engineered to be both polyethylene-like and degradable on demand, offering a possible solution to the polymer pollution problem associated with PE.98,99 Finally, this work illustrates how advances in polymer synthesis enable the preparation of previously inaccessible materials for fundamental studies and discovery of unexpected polymer properties.
| This journal is © The Royal Society of Chemistry 2025 |