Yating
Yu†
a,
Sida
Chen†
a,
Hai-Peng
Liang
b,
Ziqi
Zhao
a,
Guangze
Chu
a,
Ziting
Zhi
a,
Xian-Ao
Li
a,
Cheng
Li
a,
Ruixin
Li
a,
Xin
Liu
a,
Minghua
Chen
*a,
Youzhi
Xu
*c,
Stefano
Passerini
*def and
Zhen
Chen
*a
aKey Laboratory of Engineering Dielectric and Applications (Ministry of Education), School of Electrical and Electronic Engineering, Harbin University of Science and Technology, Harbin 150080, China. E-mail: chen.zhen@hrbust.edu.cn
bGBA Institute of Collaborative Innovation, Department of Materials and Chemical Engineering, Sino-Singapore Guangzhou Knowledge City (China), 510555, China
cCollege of Chemistry and Molecular Sciences, Henan University, Kaifeng 475004, China
dHelmholtz Institute Ulm (HIU), Ulm 89081, Germany
eKarlsruhe Institute of Technology (KIT), Karlsruhe 76021, Germany
fAustrian Institute of Technology (AIT), Center for Transportation Technologies, Giefinggasse 4, 1210 Wien, Austria
First published on 1st August 2025
Single-ion conducting copolymer electrolytes (SIPEs) have significant potential for next-generation lithium metal batteries (LMBs). However, the unsatisfactory ionic conductivity, limited mechanical strength, and lack of insights into the lithium-ion transport mechanism hinder their wide applications in LMBs. In this regard, we develop a novel SIPE through tethering lithium 3-hydroxypropanesulfonyl-trifluoromethanesulfonylimide onto a poly(vinylidene fluoride-co-trifluorochloroethylene)-based copolymer (PCL-SIPE). Molecular dynamics simulations reveal a unique transport pathway where fluorine atoms in the copolymer backbone interact with lithium-ions, serving as staging points for ion transport between adjacent sidechains. Compared with dual-ion conducting counterparts, PCL-SIPE exhibits significantly higher Young's modulus (28 vs. 17 GPa), tensile strength (20.65 vs. 5.65 MPa), and tLi+ (0.94 vs. 0.39), achieving substantially prolonged lithium stripping-plating lifetime, ca., >3200 vs. 323 h. This is predominantly ascribed to the as-formed favorable solid electrolyte interphase with ideal constitutions—ultra-high LiF content in combination with Li2O, dynamically regulating uniform Li+ flux and stabilizing the electrode|electrolyte interface. Thereby, PCL-SIPE demonstrates superior compatibility with both LiFePO4 (LFP) and LiNi0.8Co0.1Mn0.1O2 cathodes in full-cells, and achieves impressive performance even under high-loading conditions (15 mg cm−2), low-temperature (−30 °C), in trilayer bipolar stacking pouch full-cells, achieving an energy density of 245.88 Wh kg−1. These render PCL-SIPE a strong candidate for next-generation high-performance LMBs.
Broader contextThe global transition toward electrified transportation, smart energy infrastructure, and high-efficiency renewable energy storage systems is driving an urgent need for next-generation lithium metal batteries (LMBs) with higher energy density and intrinsic safety. However, the practical deployment of LMBs remains hindered by the formation of lithium dendrites, which compromise safety by piercing separators and inducing short circuits, and by the use of flammable liquid electrolytes. Single-ion polymer electrolytes (SIPEs) offer a promising pathway to address both challenges by suppressing anion-induced concentration polarization and mitigating dendrite growth through high lithium-ion transference numbers. Yet, existing SIPEs often suffer from a trade-off between room-temperature ionic conductivity and mechanical robustness. In this work, we present a molecular design strategy that covalently integrates lithium salt anions into the polymer backbone, achieving a synergistic enhancement of ionic conductivity and mechanical strength while ensuring electrochemical stability and favorable interfacial compatibility. This approach provides a new paradigm for the design of high-performance SIPEs and represents a significant step toward the realization of safe, high-energy-density LMBs. |
Polymer electrolytes, known for their improved thermal stability and mechanical properties, have garnered significant attention.8,9 Early polymer electrolytes, pioneered by Wright in 1973 using poly(ethylene oxide) matrices, demonstrated the potential of these materials.10 However, conventional dual-ion polymer electrolytes (DIPEs), where both lithium-ions and anions move freely, face limitations due to low lithium-ion transference numbers (tLi+ < 0.5).11 In DIPEs, the migration of anions is faster than that of lithium-ions, which leads to concentration gradients and dendrite growth, impeding battery performance and safety.12,13 To address these issues, single-ion conducting polymer electrolytes (SIPEs) have emerged as a promising solution. By covalently tethering anions to the polymer backbone, SIPEs achieve nearly unity lithium-ion transference (tLi+ ≈ 1), suppressing dendrite growth and improving lithium-ion transport, offering a pathway toward safer and higher-performance LMBs.14
SIPEs are known for their insufficient ionic conductivity and/or limited electrochemical stability against oxidation.15,16 To overcome the limitation of low ionic conductivity, plasticizers such as organic solvents or ionic liquids are generally introduced.17–19 Although these additives enhance ion mobility, they frequently compromise mechanical strength, leading to challenges in maintaining structural integrity during battery cycling.20,21 G. Brunklaus et al.22 synthesized a homopolymer single-ion conductor containing a polysulfonylamide segment, achieving an ionic conductivity of 0.52 mS cm−1 after blending with poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP) and incorporating a mixed solvent of ethylene carbonate and propylene carbonate (PC). While PVDF-HFP improves the film-forming ability and flexibility of the electrolyte, the trade-off between conductivity and mechanical stability remains. To overcome this issue, multi-block copolymers with tunable block sizes and constituents have been explored to balance ionic transport and mechanical strength.23 For example, based on a three-step method, Zhou et al.24 synthesized an SIPE by in situ copolymerization of lithium 1-[3-(methacryloyloxy)-propylsulfonyl]-1(trifluoromethanesulfonyl)imide and pentaerythritol tetraacrylate monomers, achieving an ionic conductivity of 2.24 × 10−3 S cm−1, a fracture stress of 4.7 MPa, and a maximum strain of 7.1%. Similarly, Nguyen25 and Chen et al.26 designed a self-standing, nanostructured SIPE based on a multi-block co-poly(arylene ether sulfone) polymer backbone, covalently attached with lithium perfluorosulfonimide side chains. After plasticization, the electrolyte achieved an ionic conductivity of 0.6 mS cm−1 at 20 °C and an electrochemical stability window of 4.96 V. However, despite their favorable properties, these materials usually involve complex synthesis procedures that pose challenges for large-scale production. Therefore, developing SIPEs that combine high ionic conductivity, high mechanical strength and ease of preparation remains a major challenge. Additionally, the lithium-ion transport mechanism, a critical factor for optimizing electrolyte performance, is still underexplored.
In this study, we designed a cost-effective SIPE based on poly(vinylidene fluoride-co-trifluorochloroethylene) copolymer, integrating –SO2–N−–SO2–, O–C–C–C, and C–F functional groups in the side chains through a straightforward synthetic process. The –SO2–N−–SO2– anion exhibits highly delocalized negative charges, promoting efficient lithium-ion dissociation. The O–C–C–C flexible group promotes segmental movement of side chains. The –CF3 end groups significantly improve thermal and electrochemical stability,27 while facilitating the formation of LiF-enriched solid electrolyte interphase (SEI). Compared with the controlled sample (denoted as PC/L-DIPE), which was prepared by simply mixing Li-salt with poly(vinylidene fluoride-co-trifluorochloroethylene) (PVDF-CTFE), this kind of design delivers superior mechanical strength, a near-unity tLi+, and a significant reduction in dendritic lithium growth. Furthermore, molecular dynamics simulations further decipher that fluorine atoms in the copolymer backbone act as staging points for lithium-ion transport between side chains, offering valuable insights into lithium-ion transport mechanisms. These properties lead to enhanced electrochemical performance in Li||Li symmetric cell, Li||LiFePO4 and Li||LiNi0.8Co0.1Mn0.1O2 full-cell configurations, showcasing PCL-SIPE as a strong candidate for next-generation LMBs.
The flatness and mechanical strength of SIPEs are critical in preventing the nucleation and growth of Li dendrites.28,29 Compared to the dry-PC/L-DIPE (Fig. S3), the dry-PCL-SIPE exhibits significantly smoother and denser surface morphology. This is further confirmed by cross-sectional scanning electron microscope (SEM) images and energy dispersive X-ray spectroscopy (EDS) analyses of dry-PCL-SIPE and dry-PC/L-DIPE (Fig. 1E and Fig. S4). The thickness of dry-PC/L-DIPE and dry-PCL-SIPE was estimated in the range of 50 ± 5 μm. The volume swelling behavior of the dry-PCL-SIPE membrane is displayed in Fig. S5. In addition, the compatibility between PC and dry-PCL-SIPE (or dry-PC/L-DIPE) is compared in Fig. S6. In the next step, the surface roughness of copolymer membranes was examined using atomic force microscopy (AFM). Evident from the representative images (5 μm × 5 μm) of the surface topography of the dry-PCL-SIPE and dry-PC/L-DIPE (Fig. 1F and Fig. S7A), their surface roughness was determined to be approximately 51.74 and 155.26 nm, respectively, in good agreement with the SEM observations. The smoother and denser structure of dry-PCL-SIPE enables better electrolyte|electrode contact and reduced interface impedance, both of which contribute positively to the battery performance. Furthermore, the dry-PCL-SIPE offers higher Young's modulus and tensile strength than the dry-PC/L-DIPE, ca., 28 vs. 17 GPa and 20.65 vs. 5.65 MPa (Fig. 1G, H and Fig. S7B and S8), respectively. The tensile strength of dry-PCL-SIPE ranks among the top reported for SIPEs in the past three years, underscoring its mechanical robustness (Fig. S9). The superior mechanical properties of dry-PCL-SIPE are primarily attributed to the chemical grafting of LiHPSI onto the PVDF-CTFE backbone. This grafting enhances the polymer network's structural integrity, allowing it to resist deformation more effectively under stress. The covalent bonding promotes a more uniform stress distribution, resulting in increased Young's modulus and tensile strength. In contrast, dry-PC/L-DIPE relies solely on a physical blending approach, where stress is not efficiently transferred between the polymer matrix and dispersed phases. This phase incompatibility limits its mechanical performance. These findings demonstrate that chemical grafting significantly outperforms simple blending in enhancing mechanical properties. While the tensile strength of PCL-SIPE decreases to 1.68 MPa due to the liquid PC uptake, the break elongation increases by approximately 16 times compared to the dry state (Fig. 1H). This observation suggests that the absorbed PC plasticizes the polymer matrix, improving its flexibility while reducing its ability to withstand higher tensile forces.
Thermal stability, a crucial factor in evaluating battery safety, was compared via conducting membrane heating and thermogravimetric analysis (TGA) tests. As shown in Fig. 1I, when heated to 220 °C, the dry-PCL-SIPE and dry-PC/L-DIPE exhibit minimal thermal shrinkage, suggesting its superiority over that of commercial separators. TGA was employed to further investigate the thermal stability and liquid uptake rate (Fig. S10 and Table S3). The dry-PCL-SIPE substantially delays the thermal lithium salt decomposition temperature from 246 °C to 331 °C, underscoring the vital role of chemical grafting in enhancing the thermal feature. As expected, incorporating the molecular transporter, PC, initiates lower onset decomposition temperature, predominantly due to its plasticizing effect reducing the crystallinity of copolymer, as revealed by the sharply decreased glass transition temperature (Fig. S11 and S12). The initial weight loss of PCL-SIPE and PC/L-DIPE occurs between 107–174 °C and 128–221 °C, respectively, and can be assigned to the evaporation of PC. The weight loss of PC in PCL-SIPE and PC/L-DIPE is consistent with the liquid uptake ratio calculated using eqn (S1). The qualitative flammability assessment of dry-PCL-SIPE, PCL-SIPE and Celgard 2325 separator (polypropylene–polyethylene–polypropylene, PP–PE–PP) with 1 M LiPF6 in EC/DEC/DMC are shown in Videos S1–S3. The results show that the dry-PCL-SIPE, representing a fully solid-state electrolyte, exhibits a self-extinguishing behavior when exposed to an open flame, indicating its excellent flame retardancy (Video S1). In contrast, the PC-containing PCL-SIPE membrane sustains combustion until the PC is consumed (Video S2), while the commercial liquid electrolyte system (1 M LiPF6 in EC/DEC/DMC) burns violently and completely (Video S3), highlighting the severe safety risks associated with liquid electrolytes.
Solid-state 7Li NMR spectroscopy was employed to further investigate the local environment and transport mechanism of lithium-ions in the electrolyte (Fig. 2E and F). Compared to the dry-PC/L-DIPE (0.73 ppm), the reduced chemical shift in the dry-PCL-SIPE (0.63 ppm) indicates an increased electron cloud density around Li+, suggesting stronger Li+-anion interactions. This enhanced interaction, however, correlates with a comparatively lower Li+ mobility,32 consistent with previous literature.33 In addition to the 0.73 ppm peak attributed to LiHPSI, three additional peaks corresponding to PVDF-CTFE interacting with LiHPSI in PC/L-DIPE are observed at 1.38, 2.41, and 3.95 ppm, respectively.
Raman spectroscopy was conducted to investigate the anion coordination, revealing that Li-ions in the dry-PC/L-DIPE are more extensively aggregated than in the dry-PCL-SIPE (Fig. 2G and Fig. S14). The radial distribution function (RDF) of Li and N atoms (Fig. 2H) further supports this observation. In the PCL-SIPE system, a single peak is observed due to the presence of only one nitrogen atom per side chain, with a coordination number of 1.4, indicating the single-ion conducting nature of the copolymer. In contrast, PC/L-DIPE shows two distinct peaks, indicating the existence of aggregates (AGGs) formed by multiple anions interacting with a Li-ion, as shown in the corresponding snapshot, and multiple Li-ions interacting with an anion for the overall charge balance. The microscopic distribution of Li+ in the PCL-SIPE and PC/L-DIPE systems was evaluated using the Li–Li RDF (Fig. 2I). The PCL-SIPE exhibits only two relatively shorter and narrower peaks, indicating a more uniform distribution of Li-ions. In contrast, the PC/L-DIPE displays two broader peaks, indicating random Li–Li interactions and confirming the existence of AGGs. This is consistent with the results from Raman spectroscopy analysis. The interaction force of Li+–anion and Li+–PC in the PCL-SIPE and PC/L-DIPE systems was evaluated using the Li–O RDF (Fig. S15 and S16). The coordination number of the PCL-SIPE system is 2.1, while that of the PC/L-DIPE system is 1.6, indicating the binding between lithium-ions and oxygen is more robust in the PCL-SIPE, with a reduced number of free Li-ions. Nevertheless, there is essentially no distinction between the Li+–O (PC) RDF of the two systems, thus, PC itself lacks analytical significance.
To further elucidate the Li+ transport mechanisms, the hopping events alongside the coordination environment were investigated, which are illustrated in Fig. 2J. In the initial stage, the Li-ion is predominantly coordinated with the anchored anion, maintaining a Li–O distance of 2.0 Å (state 1). Subsequently, the Li-ion hops to state 2 by dissociating from the anion's oxygen and hopping to the PVDF-CTFE backbone. In the third step, the Li+ ion hops to another, nearby, anchored anion forming a lithium–oxygen coordination bond with a Li–O distance of 2.0 Å (state 3), overall resulting in its migration along the alternating copolymer structure. This analysis highlights the complex dynamics of Li+ transport within the system.
The effective lithium-ion conductivities of PCL-SIPE and PC/L-DIPE were calculated to be 1.69 and 0.86 mS cm−1 (30 °C), respectively. The PCL-SIPE exhibits conductivity values comparable to those reported in the past three years34–52 (see Fig. 3C and Table S5). Additionally, the electronic conductivity of PCL-SIPE decreases by a factor of 5 (from 1.4 × 10−9 S cm−1 to 2.7 × 10−10 S cm−1) compared with the one of PC/L-DIPE (Fig. S20). Tafel plots were constructed to analyse the electrochemical reaction kinetics of the two polymer electrolytes (Fig. 3D). The PCL-SIPE exhibits higher exchange current densities (I0) and lower polarization, promoting rapid charge transfer and faster kinetics. Furthermore, as shown in Fig. 3E, the limiting current density is increased nearly by a factor of 10, i.e., 4.01 mA cm−2 (PCL-SIPE) vs. 0.42 mA cm−2 (PC/L-DIPE). In addition, the concentration gradient of PC/L-DIPE caused by the increased voltage makes the plateau different from that of the PCL-SIPE.53 These findings corroborate the significantly enhanced kinetic property of PCL-SIPEs.
To assess the stability of the Li|electrolyte interface and the effectiveness in inhibiting lithium dendrite formation, lithium stripping-plating experiments were conducted in Li||Li cells at 25 °C. The PCL-SIPE achieves higher critical current densities (CCD), i.e., 1.2 vs. 0.5 mA cm−2 in the constant-time mode (Fig. 3F), and 4.6 vs. 0.3 mA cm−2 in the constant-capacity mode (Fig. 3G and Fig. S21). Collectively, these results indicate that PCL-SIPE is capable of preventing lithium dendrite formation and ensuring sufficient kinetics even under high-power conditions. Subsequently, Li|PCL-SIPE|Li and Li|PC/L-DIPE|Li cells were subjected to long-term galvanostatic lithium stripping and plating test at 0.1 mA cm−2 (Fig. 3H). Although the Li|PC/L-DIPE|Li cell exhibits a lower overpotential, a short circuit occurs after 323 h of cycling. In contrast, the Li|PCL-SIPE|Li cell demonstrates relatively constant voltage, reaching 0.04 V after 3200 h of cycling, indicating the excellent interfacial stability and effective inhibition of lithium dendrite formation. This underscores the outstanding cyclability of PCL-SIPE, even when compared to recent studies on SIPEs (Fig. 3I and Table S6).34–37,39–52,54
Although the Nyquist plots effectively reveal differences between the two electrolytes in both the high and low frequency regions, they offer limited resolution in deconvoluting specific impedance sources. Therefore, distribution of relaxation times (DRT) analysis was employed to decouple dynamic behaviours and investigate the underlying electrochemical mechanisms (Fig. 4C–F). To perform a detailed numerical analysis, the impedance data were fitted to extract specific impedance values associated with various dynamic behaviours (see Fig. 4G–I and Table S7). The equivalent circuit model applied for fitting the DRT results is illustrated in Fig. S22. In the PCL-SIPE system, P1 (10−7 s) reflects the Li+ transport channels formed by PC and copolymer, which is closely related to the ionic conductivity of the electrolytes.55 In contrast, the presence of PC in the PC/L-DIPE system facilitates the solvation of free LiHPSI salts, thereby rendering the system liquid-electrolyte-dominated. To clarify the Li+ transport mechanism in PC/L-DIPE, we conducted theoretical calculations of Li+ RDFs in PC solvent and the PVDF-CTFE polymer matrix (Fig. S23). Results show negligible coordination between PVDF-CTFE and Li+, with extremely weak RDF peaks and near-zero coordination numbers, indicating that Li+ transport along the polymer backbone is not dominant. Therefore, in the PC/L-DIPE system, the P1 peak (10−7 s) corresponds to Li+ transport pathways primarily governed by liquid-phase conduction. This process is consistent with the overall ionic conductivity of the electrolyte. The P2 peak (10−5 s to 10−6 s) may be attributed to interfacial impedance potentially arising from the direct contact between undissociated solid-phase lithium salts and the polymer matrix. P3 (10−4 s to 10−5 s) indicates the evolution of the SEI during Li+ deposition.56 The more stable SEI layer in PCL-SIPE with respect to the PC/L-DIPE system, contributes to the superior cycling performance of the former electrolyte. P4 (10−4 s to 10−3 s) represents the charge transfer process. Rct in PCL-SIPE is higher than that in PC/L-DIPE during the whole cycling process. This behaviour is ascribed to the effective wetting of the electrode surface by solvent molecules in the PC/L-DIPE system, which enables the formation of continuous and uniform interfacial contact, thereby promoting charge transfer.
To study the surface morphology of the cycled lithium electrode, Li||Li cells were assembled, and lithium stripping-plating experiments were conducted at a current density of 0.2 mA cm−2. The voltage profiles are shown in Fig. S24. The surface and cross-sectional morphologies of the pristine lithium anode are displayed in Fig. S25. After cycling, the surface and cross-sectional morphologies, as well as the EDS mapping were also examined. Through comparison, both cycled Li electrodes present rougher surfaces, with respect to the pristine Li metal. Nevertheless, the lithium anodes cycled with PC/L-DIPE (Fig. S27) display a noticeably rougher surface, contrasting sharply with the smooth surface of those cycled with PCL-SIPE (Fig. S26). Notably, no mossy or dendritic lithium growth is seen in Li|PCL-SIPE|Li cells after cycling. Cross-sectional morphology analysis further reveals that the reactive/dead lithium layer on the cycled Li electrode recovered from Li|PCL-SIPE|Li cells is remarkably thin, indicating that PCL-SIPE facilitates more uniform lithium deposition. Additionally, the minor EDS mapping signals of cycled Li electrode recovered from Li|PCL-SIPE|Li cells further corroborate the significantly mitigated interfacial side reactions.
To investigate the SEI composition, X-ray photoelectron spectroscopy (XPS) was performed (Fig. 5A and Fig. S28). From the high-resolution F 1s XP spectra, it is seen that the SEI layer of the PCL-SIPE system contains higher amounts of LiF than that of the PC/L-DIPE system. LiF can regulate the Li+ flux and promote the uniform deposition of Li+,57 thus improving the cycle life of Li|PCL-SIPE|Li cells. The high-resolution S 2p and N 1s XP spectra reveal that the SEI layer of the PC/L-DIPE system contains higher amounts of N and S elements, attributed to increased HPSI− decomposition facilitated by the free anions reaching the electrode|electrolyte interface. The high-resolution C 1s, O 1s, Li 1s and Cl 2p XP spectra of PCL-SIPE and PC/L-DIPE are shown in Fig. S28. Notably, the LiCl peak at 56.2 eV in the Li 1s spectrum of the PC/L-DIPE system indicates the decomposition of PVDF-CTFE.
Time-of-flight secondary ion mass spectrometry (ToF-SIMS) was carried out to characterize the interphases at a time of 1000 s, with a main focus on the distribution of molecular fragments and functional groups to analyse the spatial distribution of SEI components. Depth profiling results of representative secondary ion fragments are shown in Fig. 5B and C, and Fig. S29. The sulfur (S) content in the SEI layer of the PC/L-DIPE system is remarkably higher than that of the PCL-SIPE system, indicating intensive lithium salt decomposition in the former, which is in agreement with the conclusions drawn from XPS and the possibility for the free anion to reach the electrode interface. The PC/L-DIPE shows considerably higher content of –LiO with rather uniform spatial distribution within the SEI layer. It is reported that Li2O can contribute to robust mechanical strength and enhanced interfacial kinetics.58 However, the favored LiF mainly accumulates on the surface of the SEI layer, hindering effective and uniform Li+ transport to the lithium metal. In stark contrast, the PCL-SIPE system exhibits much lower overall lithium salt decomposition and, moreover, a high content of LiF and Li2O in the bottom SEI layer. This could be assigned to the more complete decomposition of anions bound to the co-polymer and residing nearby the electrode interface, concomitantly with a higher proportion of –CF and lower –CF3. Additionally, the organic component, –C2HO, gradually decreases with increasing sputtering depth in the SEI layer of the PC/L-DIPE system, whereas an inverse trend is observed in the PCL-SIPE system. This suggests that PC decomposition intensifies in the PC/L-SIPE system, but diminishes in the PCL-SIPE system as cycling progresses.
Fig. 5D compares the 2D rendered overall distribution of total secondary ion fragments between PC/L-DIPE and PCL-SIPE systems. In the PC/L-DIPE system, the SEI components show uneven distribution due to poor compatibility between the lithium salt and the PVDF-CTFE interface, and moreover, the inhomogeneous Li deposition over cycling. Furthermore, the corresponding 3D rendering graphs (Fig. 5E and Fig. S30) more distinctly provide a visual representation of the spatial distribution of primary SEI components. Based on the above results, the SEI models are depicted in Fig. 5F and G, respectively. Compared with the SEI layer in the PC/L-DIPE system, the one in the PCL-SIPE system is denser, richer in LiF, and contains a higher content of organic components. The organic matrix mitigates interfacial stress and accommodates volume changes during cycling, thus preventing cracking or detachment of the SEI. In contrast, inorganic species such as Li2O and LiF serve to reinforce mechanical robustness and contribute to high interfacial ionic conductivity. The LiF/Li2CO3 interfacial phases can further promote the diffusion of Li+ and prevent the decomposition of the electrolyte.49 This cooperative organic–inorganic architecture facilitates stable interfacial dynamics and contributes to the prolonged cycling stability of Li metal anodes. In contrast, the absence of LiF at the bottom of the SEI layer in the PC/L-DIPE system leads to the non-uniform deposition of Li+, which will reduce the cycle life of the cells.
In order to understand the reasons behind the significantly boosted cycling performance, EIS measurements of a Li|PCL-SIPE|LFP full-cell (2 mg cm−2, 1.0C, 25 °C, 200 cycles) were performed through recording the Nyquist plots every 10 cycles. As shown in Fig. S34, the overall impedance remains rather stable after 20 cycles, indicating extremely stable interphases at both the Li|PCL-SIPE and LFP|PCL-SIPE interfaces. It is worth mentioning that the 200 cycles of dis-/charge voltage profiles of the Li|PCL-SIPE|LFP cell almost coincide (Fig. S35), an indication of excellent stability with minimized polarization. With the increase of cycle numbers, the stabilized polarization voltage gap indicates that the electrochemical reactions inside the battery gradually reach equilibrium. Furthermore, ex situ SEM and EDS analyses of cycled Li electrodes were conducted, as demonstrated in Fig. S36 and S37. Notably, no obvious dendrites are observed on the surface of the lithium metal after cycling, and the elements in the EDS mapping are evenly distributed, with no visible protrusions or cracks. Moreover, the cycled lithium metal maintains a dense structure. This suggests that the PCL-SIPE system effectively inhibits the growth of lithium dendrites during cycling.
Considering the salient advantages of PCL-SIPE in terms of ionic conductivity in low-temperature regions, fresh full-cells were subjected to galvanostatic cycling at 0.1C under various temperature conditions (Fig. 6E and Fig. S38). Between −30 °C and 20 °C, the Li|PCL-SIPE|LFP coin full-cells exhibit a reversible discharge capacity of 130.5 mAh g−1 (20 °C), 115.4 mAh g−1 (10 °C), 99.6 mAh g−1 (0 °C), 77.1 mAh g−1 (−10 °C), 54.2 mAh g−1 (−20 °C) and 33.2 mAh g−1 (−30 °C), respectively. Notably, at −30 °C, the cell retains 25.4% of the capacity achieved at 20 °C. Subsequently, the galvanostatic cycling stability of Li|PCL-SIPE|LFP coin full-cells at −30 °C is evaluated (Fig. 6F). Upon 100 consecutive cycles, the cells exhibited a capacity retention of 98.51% and an average CE of 98.78%, demonstrating its promising potential towards applications in low temperature environments.
To demonstrate the feasibility of implementing bipolar stacking cells with PCL-SIPE, “proof-of-concept” bilayer (SS|Li|PCL-SIPE|LFP|SS|Li|PCL-SIPE|LFP) coin full-cells (SS: stainless steel), denoted as CB2_Li||LFP, and trilayer (SS|Li|PCL-SIPE|LFP|SS|Li|PCL-SIPE|LFP|SS|Li|PCL-SIPE|LFP) coin full-cells, denoted as CB3_Li||LFP, were assembled. The open-circuit voltages of fresh CB2_Li||LFP and CB3_Li||LFP coin full-cells are 6.7 V and 10.1 V (Fig. S39), respectively. Fig. 6G and Fig. S40 display the discharge profiles of CB2_Li||LFP and CB3_Li||LFP coin full-cells. At 0.1C, the CB2_Li||LFP coin full-cells deliver an initial specific discharge capacity of 154.3 mAh g−1 between 8.0 V and 5.0 V. Upon cycling, the capacity initially increases and then gradually stabilizes at 164.7 mAh g−1, followed by a mild decreasing trend above 50 cycles. Impressively, to the best of our knowledge, the CB2_Li||LFP coin full-cells obtain the best cycling performance via retaining 80.0% of the maximum capacity after 150 cycles, along with an average CE of 99.65%. Furthermore, in the voltage range of 12.0–7.5 V, the CB3_Li||LFP coin full-cells deliver an initial specific discharge capacity of 139.4 mAh g−1 which progressively increases to 147.5 mAh g−1 after 45 cycles.
Li||LFP pouch full-cells (single layer pouch full-cell, PB1_Li||LFP) were assembled to explore the practical potential of PCL-SIPE with various LFP mass-loadings (Fig. 6H and Fig. S41). The initial discharge capacities of the PB1_Li||LFP pouch full-cell are 7.7 mAh (2.0 mg cm−2; Fig. 6H) and 15.0 mAh (5.0 mg cm−2; Fig. S40). The PB1_Li||LFP pouch full-cell with lower LFP loading (2.0 mg cm−2) are able to cycle more than 50 times with a capacity retention of 98.14% and average CE of 98.94%. The PB1_Li||LFP pouch full-cell with higher LFP loading (5.0 mg cm−2) deliver an initial capacity of 15.0 mAh, and retain 69.61% of the maximum capacity after 40 cycles, with an average CE of 99.34%. To further demonstrate the feasibility of PCL-SIPE for high-energy-density applications, Cu|Li|PCL-SIPE|LFP|SS|Li|PCL-SIPE|LFP|SS|Li|PCL-SIPE|LFP pouch full-cells (PB3_Li||LFP), composed of thin Li (40 μm), a high mass-loading LFP cathode (17 mg cm−2) and thin PCL-SIPE film (28 μm), were assembled (Fig. S42). According to eqn (S5), this stacking configuration successfully achieved a high energy density of 245.88 Wh kg−1 (Table S9). To assess the safety of PCL-SIPE, the PB1_Li||LFP pouch full-cell was subjected to destructive tests (Fig. S43). Due to the flexibility of PCL-SIPE, the pouch full-cells continue to operate effectively after shearing and folding. Remarkably, even after being cut into pieces, the cells can still power a light-emitting diode panel. However, the Li|PP–PE–PP|LFP pouch full-cell stopped working after shearing, reinforcing the structural and safety advantages offered by the PCL-SIPE (Fig. S44).
Finally, the combination of PCL-SIPE with high-energy Ni-rich cathode materials was investigated in Li||NCM811 coin full-cells. As shown in Fig. 6I, the Li||NCM811 coin full-cells demonstrate a high reversible specific discharge capacity of 204.0 mAh g−1 at 0.1C. Between 0.1C and 2.0C, the Li|PCL-SIPE|NCM811 coin full-cells exhibit a reversible discharge capacity of 163.2 mAh g−1 (0.3C), 142.7 mAh g−1 (0.5C) and 46.0 mAh g−1 (2.0C). After cycling at 2.0C, when the C-rate gradually reduces back to 0.1C, highly reversible capacities are delivered (Fig. 6I and Fig. S45). As shown in Fig. 6J, the Li||NCM811 coin full-cells demonstrate excellent cycling performance at 0.5C and 1.0C over 300 cycles, delivering average CEs of 99.84% and 99.54%, and capacity retention of 94.46% and 56.23%, respectively. The excellent cycling stability and rate capability of Li||NCM811 cells highlight their potential for applications requiring both high energy and high power.
Supplementary information is available. See DOI: https://doi.org/10.1039/d5ee02503f
Footnote |
† Yating Yu and Sida Chen contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2025 |