aPolymers and Functional Materials Division, CSIR-Indian Institute of Chemical Technology, Hyderabad-500007, Telangana, India. E-mail: bhosale@iict.res.in
bAcademy of Scientific and Innovative Research (AcSIR), Ghaziabad-201002, Uttar Pradesh, India
cMaterials Research Laboratory, Department of Physics, Indian Institute of Technology Jammu, Jagti, NH-44, PO Nagrota, Jammu, J&K 181221, India. E-mail: rahul.salunkhe@iitjammu.ac.in
dDepartment of Industrial and Materials Science, Chalmers University of Technology, Göteborg, SE-412 96, Sweden
eDepartment of Chemistry, School of Chemical Sciences, Central University of Karnataka, Kalaburagi-585 367, Karnataka, India. E-mail: bsheshanath@gmail.com
First published on 12th January 2024
Organic materials capable of undergoing oxidation and reduction reactions are attracting attention as potential electrode components, providing a more environmentally sustainable alternative for lithium-ion batteries (LIBs). Despite notable achievements at the laboratory level, these materials still face challenges, such as high solubility in electrolyte solutions and limited thermal stability, leading to capacity degradation. While carbon remains the benchmark for anode materials, issues like irreversible capacity loss and low specific capacity impede the development of advanced LIBs. This study presents a composite material incorporating naphthalene diimide nitro derivatives (NDI-2NO2 and NDI-4NO2) into reduced graphene oxide (rGO) as an anode material for LIBs. The inclusion of rGO not only addresses the problem of material dissolution in the organic electrolyte, but also significantly improves the rate performance and conductivity of the resulting composite materials. Specifically, at a current density of 50 mA g−1, the NDI-4NO2/rGO composite demonstrates a remarkably high specific capacity of 699 mA h g−1, while the NDI-2NO2/rGO composite yields a specific capacity of approximately 560 mA h g−1. Finally, we showcase that optimal performance as superior anode materials can be achieved by effectively combining organic compounds capable of participating in oxidation and reduction reactions with graphene-based composites.
Moreover, research efforts have been dedicated to discovering sustainable alternatives to conventional graphite anodes13–15 that offer improved energy and power density. As a result, a wide range of alloy-based materials (such as Sn, P, Ge, Si, Bi, and Sb) and transition metal oxides (including MxOy, where M represents Ni, Mn, Fe, Cr, Mo, Co, Nb, etc.) have been extensively investigated as potential anode materials for LIBs, thanks to their high specific capacity.16–18 However, these materials’ electrochemical instability and rapid capacity degradation hinder their widespread commercial application as anode materials in LIBs. For example, silicon anodes can offer ten times the capacity of graphite (3580 mA h g−1). However, the severe volumetric change (300–400%) during the lithiation causes mechanical failure and instability of the solid electrolyte interface (SEI) layer.19,20 On the contrary, transition metal oxide anodes possess high capacity (600–1000 mA h g−1) but have low coulombic efficiency and large potential hysteresis.21,22 Transition metal chalcogenides are another interesting anode material with high theoretical capacity. However, the significant alterations in the bulk material dimensions during charging/discharging generally hamper their poor cycling stability and rate capabilities.23,24 Conversely, MXenes, an emerging class of materials, have also been utilized as the anode. The low specific capacity and restacking characteristics of MXenes has limited their practical application in LIBs.25,26 Most of these drawbacks of different materials can be addressed systematically by compositing them with carbon materials, including carbon nanotubes, reduced graphene oxide (rGO), and other porous carbon materials.20,21 For example, including the carbon matrix into the silicon effectively managed the volumetric variations of silicon while preserving the electrodes’ structural integrity and electrical stability.27,28 Although, after a significant advancement in the anode materials, most of these materials employed in commercial LIBs rely on graphite materials having limited capacity (about 300 mA h g−1) for commercial applications.29,30
Up to now, the redox-active organic electrode materials,31 conducting polymers,32,33 and organic carbonyl compounds34 have been widely employed as anode materials in rechargeable LIBs.1,35 To avoid unwanted dissolution of organic materials in the electrolyte solution, strategies such as designing and constructing molecular architectures with stable and redox-dependent functional groups have been previously adopted.1,32–37 Different organic materials, including dilithium terephthalate and diethyl terephthalate,38 Li-salt derived from 1,2,4-benzene tricarboxylic acid,39 and organic compounds with nitro-containing groups like 2,2′-azobis(2-methyl propionitrile) and 2,2′-azobis(2-methylpropionamidine)dihydrochloride40 have been utilized in the literature. The key challenges associated with these molecules are the low-capacity values and their lower cycling stability.
Furthermore, to address this issue, different organic molecules utilizing bare naphthalene diimides (NDIs) and their composites have been reported in the literature,41–46 as shown in Fig. 1(a)–(g). NDIs are π-conjugated aromatic molecular chromophores bearing n-type semiconducting properties.47 Their ease of structural modification, thermal stability, and ability to incorporate redox-active functional groups,48 and to accept electrons are beneficial to tune the material properties. Towards this effort, Vadehra et al.46 reported the importance of various core substitutions on NDI molecules and their effect on the redox potential window. Furthermore, Stoddart and co-workers44 reported the rigidity of the NDI molecule and its effect on the cathodic properties for LIBs. Also, different nitro organic compounds were utilized as a cathodic electrode material in LIBs to enhance the potential window.49 Ye et al. recently explored p-, o-, and m-dinitrobenzene (DNB) compounds as cathode materials in LIBs.50 For as-fabricated LIBs, they observed that p-dinitrobenzene exhibited a reversible capacity of 535 mA h g−1 at 50 mA g−1 (average potential of 2.7 V). However, due to the high solubility of organic scaffolds, such as p-DNB, the capacity of LIBs gradually dropped to 54% after 50 cycles. Recently, Zhang et al. reported an organic cathode material based on nitro compounds.49 They demonstrated that incorporating multiple nitro-functional groups in organic molecular architectures efficiently reduced the solubility in the electrolyte solution and exhibited a high specific capacity of about 180 mA h g−1.
Fig. 1(h)–(j) show different nitroaromatics reported in the literature.49,50 Although NDIs41,43,45–48 and nitroaromatic49–51 based small molecular cathode materials in LIBs show significant advantages with a high specific capacity, there are no reports available in the literature about the use of NDI-nitroaromatics and rGO nanocomposites as anodes in LIBs.
The inherent properties of NDI molecules, such as their ability to undergo π–π aromatic stacking, make them highly suitable for electron transfer and diverse design architecture, rendering them ideal candidates for LIBs. In order to further enhance their electrochemical properties, we have introduced nitro substitutions on the NDI moieties, specifically NDI-2NO2 and NDI-4NO2. One of the challenges faced in utilizing organic materials in LIBs is their tendency to dissolve in the electrolyte.50 To address this issue, we have proposed immobilizing organic materials onto solid substrates, which offers a feasible solution to overcome the dissolution problem. Our research successfully incorporated NDI-2NO2 and NDI-4NO2 with rGO through non-covalent interactions. The π–π interaction between NDI and rGO further enhances the material's suitability for LIBs. Additionally, electron-withdrawing nitro groups appended on the NDI ring increase the electron-deficient nature, whereas rGO also serves as an electron acceptor.45 These combined characteristics make our approach scientifically sound and promising for developing high-performance LIBs.
Here, we report the LIB performance from rGO with NDI-phenyl dinitro (NDI-2NO2) and NDI-phenyl tetra-nitro (NDI-4NO2), organic architectures fabricated from NDI, p-nitro aniline (pNA) and 3,5-meta-dinitro aniline (3,5-dNA), respectively. The NDI-4NO2/rGO sample exhibited a high specific capacity of about 699 mA h g−1 at 50 mA g−1. In addition, the material shows an outstanding cycling stability of 800 cycles with minimal fading. Our investigation has explored the redox mechanism of NDI-2NO2/rGO and NDI-4NO2/rGO and the potential of incorporating nitroaromatic functional groups into NDI compounds to develop better anode materials for LIBs.
C (3081, 3088 cm−1), –C
O (1714 cm−1), –C
C (1580, 1536 cm−1), etc. (Fig. S1, ESI†). Furthermore, 1H NMR spectra of NDI-4NO2 showed the presence of a proton peak designated as ‘a’ at 9.01 (m, 2H); additionally, a proton peak labelled as ‘b’ appeared at 8.96 (d, 4H), and another proton peak labelled as ‘c’ emerged at 8.82 (s, 4H) (Fig. S2, ESI†). Similarly, 1H NMR spectra of NDI-2NO2 showed the appearance of an ‘a’ labelled proton peak at 8.76 (s, 4H) and ‘b’ labelled proton peak at 8.47–8.44 (d, 4H), and a proton peak labelled as ‘c’ appeared at 7.83–7.81 (dd, 4H), as displayed in Fig. S3 (ESI†), which confirmed the formation of NDI-2NO2 and NDI-4NO2 molecules. Furthermore, the HRMS spectrum of NDI-4NO2 indicates a good agreement between the m/z calculated for C26H12O8N4: 598.03512, and the experimental value: [M]+ 598.03400 (Fig. S4, ESI†). Similarly, the HRMS spectrum of NDI-2NO2 indicated a good agreement between the calculated and experimental values (Fig. S5 (ESI†); m/z [M]+ calculated for C26H12O8N4: 508.06536, experimental: 508.06496). The as-prepared organic molecules were soluble in organic solvents, making it difficult to use them as the anode material in the presence of organic electrolytes. Hence, they have been composited with rGO. The self-assembled composite formation with rGO is a practical design strategy to suppress the dissolution of NDI derivatives in organic electrolytes.52 During the composite formation, the interaction between NDI and rGO may enhance the electron transfer rate, impacting the composite material's high cycling stability, similar to the previous report.53 Notably, the functional groups such as C
O, C
C and C–O–H in rGO can be advantageous for binding with organic materials.
The schematic representation of the synthesis process for NDI-4NO2/rGO and NDI-2NO2/rGO materials is shown in Scheme 1. Co-precipitation of NDI-2NO2, NDI-4NO2, and graphene oxide (GO) was utilized for obtaining composite materials. Hydrazine hydrate (NH2NH2) helped reduce GO to rGO. Further details of the synthesis process can be found in the Experimental section and Note S1 (ESI†). The thermal stability of rGO, NDI-2NO2/rGO, and NDI-4NO2/rGO under a nitrogen environment was determined using thermogravimetric analysis (TGA). Measurement was performed using a TA instrument Q500 TGA under flowing nitrogen gas at a heating rate of 10° min−1 up to 800 °C. As shown in Fig. S6 (ESI†), the TGA results reveal that bare rGO, NDI-2NO2/rGO, and NDI-4NO2/rGO displayed 5% water loss between temperatures of approximately 300 °C due to thermal decomposition. These TGA results suggest that the composites NDI-2NO2/rGO and NDI-4NO2/rGO are thermally stable and can be utilized for energy storage applications.
O, C
C, and C–O–H stretching vibrations.55 The FTIR spectra of NDI-2NO2/rGO exhibited peaks of about 1700 cm−1 attributed to the stretching vibration of the imide C
O group. Moreover, the two peaks at 1565 and 1412 cm−1 correspond to the stretching vibrations of the –NO2 functional group.50 The peaks that appeared at 870 and 755 cm−1 can be ascribed to the C–H bending vibrations.56 The presence of peaks at 1644, 1412, and 1242 cm−1 was attributed to C
O, C
C and C–O–H bonding in the rGO in the sample.57 Similar peaks were observed in the NDI-4NO2/rGO sample. Thus, the comprehensive FTIR study confirmed the successful synthesis of composite materials. Moreover, UV-vis absorption studies were performed on a UV-vis-1800 Shimadzu spectrometer, and the results are depicted in Fig. 2b. The sample rGO showed an intense absorption peak at 270 nm,57 while there is a small absorption peak for NDI-2NO2 at 264 nm (imide substituted phenyl ring system), along with one shoulder peak at 338 nm and two intense peaks at 356 and 377 nm.57 The absorption peaks ranging from 300 to 400 nm are typical of the NDI subunits and are unaffected by imide substitution.58 The NDI-4NO2 molecular architecture showed an intense absorption peak at 268 nm (phenyl ring system) and a broad peak ranging from 330 nm to 370 nm corresponding to the NDI core. Moreover, the absorption curves of the NDI-2NO2/rGO and NDI-4NO2/rGO composites exhibited peaks at 269 nm, 338 nm (shoulder), and two intense peaks at 356 nm and 377 nm, suggesting the complex formation. The intense peak at 269 nm (due to π–π transition) is the characteristic graphene peak indicating the presence of rGO in the NDI-2NO2/rGO and NDI-4NO2/rGO composites.59 Furthermore, the organic molecule's composition with rGO was investigated using Raman spectroscopy on the Horiba Jobin–Yvon Lab Ram HR spectrometer with an excitation wavelength of 632.8 nm. Fig. 2c shows that different samples exhibited characteristic peaks at 1333 and 1600 cm−1, corresponding to the D and G bands.60 The ID/IG ratio for the bare rGO sample was calculated to be 1.4, which increased to 1.44 for NDI-2NO2/rGO and 1.24 for the NDI-4NO2/rGO samples, respectively. The decreased ID/IG ratio indicates a higher degree of graphitization for the NDI-4NO2/rGO sample.61 The crystallographic structures of the rGO, NDI-2NO2/rGO, and NDI-4NO2/rGO composites are further verified by powder X-ray diffraction (P-XRD) measurements recorded on a Bruker AXS D8 (λ = 1.54 Å), and the results are depicted in Fig. S7 (ESI†). The bare rGO sample exhibited two diffraction peaks around 25° and 44°, corresponding to the standard graphite 2H phase. The composite NDI-2NO2/rGO exhibited four peaks around 13, 26.5, 29.5, and 43.5, whereas NDI-4NO2/rGO displayed peaks at about 12.8, 26.4, and 43 degrees.62 The composites NDI-2NO2/rGO and NDI-4NO2/rGO exhibited higher crystallinity than rGO, indicated by the sharp and enhanced peaks. The diffraction peaks moving towards high angles indicate that the π–π stacking between NDI moieties, such as NDI-2NO2 and NDI-4NO2, and the rGO surface was enhanced.63
Furthermore, the elemental content and the bonding conditions of the NDI-2NO2/rGO and NDI-4NO2/rGO composites were examined by X-ray photoelectron spectroscopy (XPS) measurements (Model Nexa from Thermofisher Scientific). The XPS survey spectra displayed in Fig. S8 (ESI†) exhibit the presence of carbon (C), oxygen (O), and nitrogen (N) elements only. The high-resolution narrow region spectra for various samples are shown in Fig. 2d–f. The deconvoluted spectra for the C 1s spectrum of NDI-2NO2/rGO and NDI-4NO2/rGO (Fig. 2d) can be fitted into four types of peaks located at 287.3 eV (O–C
O), oxygen and nitrogen bridged carbon (O–C and C–N) at 285.6 eV, carbon bridged carbon (C–C) at 284.8 eV and graphitic carbon (C
C) at 284.2 eV.64 Also, the high-resolution N 1s XPS spectrum for both composite samples (Fig. 2e) is dominated by two well-resolved peaks at 400.3 eV and 399.2 eV, corresponding to N–C
O and –N–C, respectively.65 Moreover, the O 1s spectrum of NDI-4NO2/rGO could be divided into two fitting peaks at 533.6 eV and 531 eV corresponding to carbon bridged oxygen C–O bonds and C
O bonds, respectively.60 Similar peaks were also confirmed for the NDI-2NO2/rGO sample (Fig. 2f). The XPS results of the NDI-2NO2/rGO and NDI-4NO2/rGO composites revealed that the nitrogen and oxygen content of the nitro functional groups dominated the composite. Tables S1 and S2 (ESI†) show the atomic percentage of C, N and O for NDI-2NO2/rGO and NDI-4NO2/rGO, which aligns with the EDS data.
The N2 adsorption/desorption isotherm was performed at 77 K to further investigate the surface area and pore size distribution. The analysis was performed on an Autosorb-iQ (Quantachrome) at 77 K. The comparative isotherms for both materials are shown in Fig. S12 (ESI†). The steep adsorption isotherm at the low-pressure region of both composites was observed, indicating the typical type IV behavior.66 The estimated Brunauer–Emmett–Teller (BET) surface area of the NDI-2NO2/rGO and NDI-4NO2/rGO composite is 34.7 m2 g−1 and 41.1 m2 g−1, respectively. The average pore diameter for NDI-2NO2/rGO and NDI-4NO2/rGO was observed to be 3.2 nm and 3.0 nm, respectively (Fig. S12b and d, ESI†). Thus, it confirms the presence of various pores in these materials. The BET surface area, pore diameter, and pore volume of NDI-4NO2/rGO are higher than that of NDI-2NO2/rGO, indicating that the former composite may provide comparatively good electrochemical performance.
The kinetics of Li+ were investigated using EIS measurement by applying alternating current with an amplitude of 5 mV with frequency ranging from 10 mHz to 100 kHz. Fig. 3d shows a comparative Nyquist plot of the NDI-4NO2/rGO and the NDI-2NO2/rGO. The inset in Fig. 3d shows the simulated Randles circuit, which fits in with the experimental data. The NDI-4NO2/rGO sample has less electrode resistance (21.3 Ω) than the NDI-2NO2/rGO sample (31.1 Ω). Also, the charge transfer resistances (Rct) of NDI-4NO2/rGO and NDI-2NO2/rGO are 36.2 Ω and 45.3 Ω, which reveals a low resistance path for Li+ ions in the NDI-4NO2/rGO sample. The CV and EIS were conducted for bare rGO for comparison shown in Fig. S14 (ESI†), which reveals that the Rct of rGO is 7.2 Ω, contributing to the high conductivity and low resistance path for the NDI samples.
The LIB coin cell composed of NDI-4NO2/rGO was further evaluated by capacity retention tests, and cyclability and diffusion studies. For the capacity retention test, current rates ranging from 50 to 5000 mA g−1 were applied and the specific capacities are shown in Fig. 4a. The cell shows some electrochemical changes during the first cycles, which gives a stable performance. The LIB cells composed of NDI-4NO2/rGO exhibited specific discharge capacities of 699, 498, 389, 325, 296, 263, 216 and 155 at current rates of 50, 100, 300, 500, 700, 1000, 2000 and 5000 mA g−1, respectively. The cell exhibits a stable performance at low as well as high current. Furthermore, the cyclability of the cells was tested for 800 cycles at a current rate of 1000 mA g−1; the device has demonstrated excellent stability, retaining about 89% of its initial capacity, as shown in Fig. 4b. The coulombic efficiency of the LIB cell was above 95% throughout the cycling, revealing very low hysteresis during charge–discharge. To present a comparative analysis of the NDI-2NO2/rGO LIB cell, its cycling tests were conducted for 500 cycles at 1000 mA g−1, which retained about 74% of its initial capacity. One of the reasons which govern the outstanding performance of NDI-4NO2/rGO is the increased nitrogen content, specifically the pyridinic type (as discussed in the XPS Characterization section) content with the highly π-conjugated structure and higher specific surface area.71
The diffusion study of Li+ ions into the host materials was studied using the galvanostatic intermittent titration technique (GITT). During the study, the charge–discharge pulse of 10 min was applied, followed by a resting period of 30 min. The diffusion coefficient (D) was calculated by eqn (2), Note S2 (ESI†). The GITT charge–discharge profile and corresponding D values are plotted as a function of time, as shown in Fig. 4c and d. During the charging, the D value increases from 2.6 × 10−13 cm2 s−1 to 1.01 × 10−11 cm2 s−1.
In contrast, during discharging, the D value is constant when it is above 0.5 V. Still, it increases rapidly in the region when the discharge curve is below 0.5 V. The high value of D manifests the fast diffusion of Li+ ions into the host material. Hence, these electrochemical studies show that the NDI-4NO2/rGO can be successfully employed as an anode material for LIBs. Along with the superior anodic performance, this cost-effectiveness, greener synthesis route of this material, and its non-solubility within electrolyte, give an upper hand over various traditional organic materials, as listed in Table S3 (ESI†).
The coin cell (CR 2032) was packed by using the 16 mm active electrode disks, lithium chips (16 mm) as a counter electrode, Whatman filter paper of grade-1 as the separator, and LiPF6 in EC
:
DMC (1
:
1) in the PC electrolyte. The cell was packed with the help of a crimper and kept at room temperature for 12 h for thermodynamic equilibrium attainment and proper electrolyte wettability.
Footnotes |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3ya00561e |
| ‡ These authors contributed equally to this work. |
| This journal is © The Royal Society of Chemistry 2024 |