S. no | Material | Preparation method | Optimized calcination temperature (°C) | Optimized sintering temperature (°C) | Relative density % | Dielectric properties | Ref. | ||
---|---|---|---|---|---|---|---|---|---|
ε r | Q × f (GHz) | τ f (ppm per °C) | |||||||
1. | MgTi0.98O2.96 | Solid state | 650 | 1120 | 95.2 | 16.45 | 48![]() |
−48 | 17 |
2. | MgO + TiO + CaO | Solid state | 1100/2.5 h | 1310/4 h | 96 | 21.1 | 86![]() |
−3.8 | 21 |
3. | 0.95MgTiO3–0.05CaTiO3 | Solid state | 1000 | 1450 | 96.4 | 20.1 | 68![]() |
1.81 | 22 |
4. | 0.935MgTiO3–0.065CaTiO3 + 5 wt% ZnNb2O6 | Solid state | 1100/3 h | 1300/2h | 97 | 22.5 | 93![]() |
6.2 | 23 |
5. | MgZrNb2O8 | Solid state | 1200/4 h | 1340/4 h | 98 | 26 | 120![]() |
−50.2 | 26 |
6. | 0.3MgTiO3–0.6Mg2TiO4–0.1(Ca0.7La0.3)(Ti0.7Al0.3)O3 | Solid state | — | 1230 | — | 18 | 51![]() |
−4.6 | 45 |
7. | 0.96MgTiO3–0.04SrTiO3 | Solid state | 1100/3 h | 1350/3 h | — | 18.74 | 26![]() |
1.76 | 46 |
8. | MgTiO3–15 wt% B2O3 | Solid state | — | 200 | 96 | 14.5 | 39![]() |
−54.39 | 47 |
9. | 0.78Mg6Ti5O16–0.22Ca0.8Sr0.2TiO3 | Solid state | 1100/4 h | 1400/4 h | 96 | 20.25 | 74![]() |
−1.28 | 48 |
10. | MgTi0.99(Mn1/2W1/2)0.01O3 | Solid state | 1100/3 h | 1325/4 h | 99 | 18.74 | 160![]() |
−58.2 | 49 |
11. | MgZr0.9Ti0.1Nb2O8 | Solid state | 1100/3 h | 1320/4 h | — | 25.72 | 130![]() |
−46.60 | 50 |
12. | MgTiO3 | Solid state | 1000/4 h | 1500/4 h | 97.18 | 18.2 | 103![]() |
−45.23 | Present work |