Open Access Article
Maotao Huanga,
Jianwen Zhanga,
Xianlan Kea,
Shuai Gaob,
Dimeng Wub,
Junying Chen*a and
Yajun Weng
*a
aKey Laboratory of Advanced Technologies of Materials, Ministry of Education, School of Materials Science and Engineering, Southwest Jiaotong University, Chengdu, PR China. E-mail: chenjunying@swjtu.edu.cn; wengyj7032@swjtu.edu.cn
bChengdu Daxan Innovative Medical Tech. Co., Ltd, Chengdu, PR China
First published on 17th January 2022
Nitric oxide (NO) shows high potential in the cardiovascular system with anticoagulant and antibacterial efficacy. Cu based metal organic frameworks with amino modification (CuMOFs) were found to have an extraordinary high NO loading, but at the expense of framework stability in ambient moisture. Nano CuMOFs was synthesized by hydrothermal method in this work, and treated with stearic acid (SA) creating a hydrophobic form. It was found that the structure of the particles was not affected after treatment with SA, and the treated CuMOFs had tunable hydrophobicity. Both CuMOFs and SA modified CuMOFs adsorbed NO with the reaction of the amino group and NO to form a NONOate. SA modification enhanced stability of the CuMOFs in phosphate buffer solution (PBS, pH = 7.4), slowed down the interaction between the NO loading unit and H2O, and thus NO releasing was prolonged. The resulting NO-loaded CuMOFs inhibited platelet activation dramatically, prolonged the coagulation time and displayed excellent antibacterial properties. They could be envisioned as a good candidate for application in blood contacting implants.
NO delivery technologies using solid storage materials are increasingly significant. Examples of NO carriers currently investigated mainly include NONOates,11,12 metal exchanged zeolites,13 and metal–organic frameworks (MOFs).14 NONOates were among the first compounds to be studied for potential NO delivery, and are molecular species capable of releasing chemically bound NO upon contact with water. Alternatively, one of the most promising candidates for NO delivery is currently the use of porous materials, especially MOFs. MOFs represent a class of hybrid organic–inorganic porous materials that have attracted a lot of interest because of their chemical tunability, high porosities, and good thermal stability. They can be activated in vacuum at high temperature to obtain coordinatively unsaturated metal sites (CUSs) on the walls of the pores, which are available for binding of small molecules. Among the various MOFs, CuBTC (also known as HKUST-1) is one of the highly studied MOFs with CUSs, for which applications in NO delivery have been demonstrated.15 Recently, the amino functionalized MOF, Cu3(NH2BTC)2 (ref. 16) was used to load NO which showed NONOate formation additional to the coordination of NO to unsaturated copper centers.17
However, one of the major shortcomings of MOFs is their instability in the presence of moisture, and some researchers tried to enhance its stability in water or PBS. For example, a modified CuBTC with plasma enhanced chemical vapor deposition of perfluorohexane was reported by Decoste et al. to prevent the formation of water clusters around the Cu sites.18 Rani et al. reported that HKUST-1 post-synthetically modified with amino acids showed transition behavior from hydrophilic to hydrophobic, and thus had better stability in aqueous environment.19 Moreover, for enhancing hydrophobic small molecule capture, materials or solvents were tailored for increased hydrophobicity.20–22 To obtain a sustained NO release, Mondal et al. reported a highly hydrophobic polytetrafluoroethylene particle immobilization on NO releasing polymer to slow down interaction of NO releasing polymer with water molecules.23
In this study, Cu based MOFs was tailored with amino group and SA modification to obtain a super hydrophobic form and sustained NO release (Fig. 1). A hybrid linker coordinated CuMOFs was first prepared by hydrothermal method, which had amino group as a functional group to form NONOates when contacting NO. Then it was post-synthetically modified with stearic acid (SA) to obtain hydrophobic/super-hydrophobic properties. Copper ion and NO release, and anticoagulant and antibacterial properties in vitro were evaluated.
:
10) was added subsequently. Then it was ultrasonically treated for 20 min to obtain CuMOFs precursor solution. The precursor solution was kept in an autoclave for 1 h at 140 °C. After being taken out, the sample was centrifuged at 4000 rpm for 5 min, then washed two times with ethanol and dried at 80 °C for 5 h to get the final CuMOFs nanoparticles.
400 mg of CuMOFs was dispersed in ethanol solution, and SA was added to obtain a final concentration of 0 mg mL−1, 0.625 mg mL−1, 2.5 mg mL−1 and 10 mg mL−1 respectively. After being ultrasonically treated for 30 min, the samples were centrifuged at 12
000 rpm for 10 min and dried for 5 h at 80 °C. The obtained samples were referenced to as SA1@CuMOFs, SA2@CuMOFs, SA3@CuMOFs which represented SA concentration of 0.625 mg mL−1, 2.5 mg mL−1 and 10 mg mL−1 respectively.
NO release was measured using the total NO assay kit. NO can be easily transferred into nitrite and nitrate in water. For total NO assay, nitrate in the solution was reduced to nitrite by nitrate reductase and the total nitrite was quantitatively detected by classical Griess reagent. Details was as follows. First, 1 M NaNO2 was diluted with PBS to 2, 5, 10, 20, 40, 60 and 80 μmol L−1 to get a standard curve. Second, 100 mg of NO@CuMOFs and NO@SA3@CuMOFs was placed into the prepared dialysis tape respectively, and then incubated in 100 mL PBS at 37 °C. At each of the preset time, the solution was analyzed for NO release according to the total NO assay kit.
For coagulation time test, 500 μL fresh whole blood without anticoagulant and 10 mg of CuMOFs or NO@SA3@CuMOFs were simultaneously added into a 24-well cell culture plate. After incubation for a preset time (20 min, 40 min and 60 min) at 37 °C, 2 mL of physiological saline was added. The coagulated clots will precipitate and 50 μL supernatant was transferred to a new plate. After 2 mL of physiological saline was added, absorbance at 545 nm was detected.
The antibacterial potency of CuMOFs, NO@CuMOFs and NO@SA3@CuMOFs against E. coli and S. epidermidis was investigated by the minimal inhibitory concentration estimation and growth inhibition assay. The minimal inhibitory concentration of NO@SA3@CuMOFs was evaluated as follows. The optical density (OD) of the cultures was adjusted to 0.2 at a wavelength of 600 nm (1.5 × 108 CFU mL−1). Samples was first diluted with saline into series of concentration, and 10 mL of the series of diluted solution and 10 mL of agar medium was added into a Petri dish. After solidification, 2 μL of bacterial suspension was seeded and then incubated in a bacterial incubator at 37 °C for 24 hours. The minimal inhibitory concentration was determined by the highest dilution showing complete inhibition of the tested strain. For growth inhibition assay, the pre-cultured E. coli and S. epidermidis were diluted 100 times to obtain a test inoculum with a concentration of 1.5 × 106 CFU mL−1 5 mL of the test inoculum was added into a tube, then 12.5 mg samples were added. After incubation at 37 °C for 24 hours, the surviving bacteria were collected into a new Petri dish by washing with 10 mL sterilized saline. Then 30 μL of 1.5 × 105 CFU mL−1 inoculum was seeded on agar to count the colonies after 24 h culture. The antibacterial rate was calculated according to the following formula
![]() | (1) |
The CuMOFs and SA modified CuMOFs were dispersed in ethanol and a uniform coating was prepared on titanium foil by dipping and pulling for 5 times. Water contact angle was detected and it showed the surface with CuMOFs was superhydrophilic. The topography of the microstructure of the nanoparticle combined with surface charge of Cu(II) may both contributed to the super wettability. Whereas surfaces SA1@CuMOFs, SA2@CuMOFs, and SA3@CuMOFs presented hydrophobic and superhydrophobic behavior with the contact angles of 62°, 109°, and 154° respectively (Fig. 2b). To reduce the interaction between water and the loaded NO cargo in the nanoparticles, SA3@CuMOFs with superhydrophobic properties was chosen for the following studies.
FTIR spectra were recorded for the studied nanoparticles before and after SA modification. The distinct changes in FTIR spectra after SA modification are discussed below. The two characteristic peaks at 2919 and 2853 cm−1 assigned to C–H stretching of SA were apparently increased (Fig. 2c).25 Vibration of functional group –NH2 was overlapped with –OH of carboxylic group, which formed a wide absorption instead of a sharp peak around 3400–3500 cm−1 for both samples.
The crystallographic structure of the as-prepared samples is analyzed by powder X-ray diffraction (XRD). The X-ray diffraction (XRD) results showed significant diffraction peaks within 5–50° of 2θ and the position and relative intensity of the diffraction peaks of SA3@CuMOFs and NO@SA@CuMOFs were mainly consistent with the typical HKUST-1 (ref. 26) (Fig. 2d). The CuMOFs has extremely intense diffraction peaks at 6.7°, 9.6°, 11.6° and 13.5°, which correspond to the (200), (220), (222), (400) lattice planes of HKUST-1 respectively. However, the other diffraction peaks of HKUST-1 at 16.6°, 19.1°, 24.3°, 26.1°, 29.5° and 35.5° are very weak, which correspond to the (422), (440), (220), (551), (731), (751), (951) planes, respectively.27 There was rarely little change compared with the simulated HKUST-1, indicating the CuMOFs and SA modified CuMOFs were HKUST-1 liked crystallographic structure.
N stretching of the NONOate group.28 Furthermore, a shift of absorbance at 940 cm−1 to 932 cm−1, and the shoulder at 1683 cm−1 increased and sharped after NO loading. The signal around 1683 cm−1 is a characteristic of a –N
N–O group and therefore would indicate the formation of NONOate groups inside the MOFs.16 The FTIR results indicated CuMOFs and SA3@CuMOFs both can load NO via NONOate formation.
For sustained NO release, the stability of CuMOFs in PBS is critical. The CuMOFs and SA3@CuMOFs were incubated in PBS for preset times, and Cu2+ ions concentration was measured. From the experimental results of Fig. 3c, the degradation rate of SA3@CuMOFs in aqueous solution for the first 7 days was significantly decreased. The superhydrophobic property of SA3@CuMOFs reduced the interaction between water and the MOFs to some extend, and delayed the degradation compared with that before SA modification.
NO release was shown in Fig. 3d. It can be seen that the bare CuMOFs particles loading with NO can release for about 72 h. After 72 h, the NO release of NO@CuMOFs is significantly slowed down and nearly not released. A total of 1.19 mmol of NO was released per gram of NO@CuMOFs. For NO@SA3@CuMOFs, although there was no significant difference for the first three days, however, it kept sustained NO release for 7 days. The cumulative release amount was 1.52 mmol per gram. It indicated SA may have the role of solubility enhancement of NO via hydrophobic interaction thus the loading amount increased.
The release time is one of concerned performances in the research of NO releasing materials. Many researches focused on improving the release time of NO. The comparison of the performance of NO releasing MOFs was showed in Table 1. It can be seen that NO@SA3@CuMOFs investigated herein offer the highest released amount with a sustained NO release about 168 h. The duration of NO release mainly depends on two factors. One is the stability of the frameworks, the other is the reaction rate of NO loading unit with H2O. In the present study, SA modification not only enhanced the stability of the frameworks but also slowed down interaction of NO loading unit with water molecules. Both contributed to the long NO duration.
| Material | Release conditions | Released amount | Duration of NO release | Ref. |
|---|---|---|---|---|
| CuMOFs | PBS | 1.19 mmol g−1 | ∼72 h | This work |
| NO@SA3@CuMOFs | PBS | 1.52 mmol g−1 | ∼168 h | This work |
| UiO-66-NH2 | PBS/acid | 1.1 mmol g−1 | ∼4 h | 29 |
| HKUST-1 | 11% relative humidity | 0.001 mmol g−1 | Nearly complete after 20 min, continues for up to 60 min | 30 |
| Cu-TDPAT (diazeniumdiolated MOF) | 85% relative humidity, room temperature | 0.175 mmol g−1 | Initial burst in the first 3 h, then continued slower release in 168 h | 31 |
| NOF-11 (with bis-N-nitroso) moiety | Light irradiation | 1.0 mmol g−1 | 3600 s | 32 |
| MIL-100 (Fe) | 11% relative humidity, 200 mL min−1 | 0.55 mmol g−1 | Primarily released in first 2.5 h continues up to 25 h | 33 |
| UHM-37 | 11% relative humidity | 0.0644 mmol g−1 | ∼6 h | 34 |
We tested the anticoagulation property of the as synthesized nanoparticles in vitro. Platelet adhesion on cell culture plate well was done, and samples were added in a Millipore transwell chamber which incubated within the PRP. As shown in Fig. 4a, the morphology of adhered platelets in both the blank and the CuMOFs groups displayed a spreading and fully spreading state, and the activation degree in the CuMOFs group was more pronounced. In contrast, most adhered platelets in the NO@CuMOFs and NO@SA3@CuMOFs groups kept round or a little spreading state, which indicated that NO release from the samples and acting as an important platelet activation inhibitor. According to the statistics of activation rate, about 87% of the adhered platelet were activated in the blank group, while only 20% and 18% were activated with NO@CuMOFs and NO@SA3@CuMOFs incubation respectively. But there is no significant difference in NO@CuMOFs and NO@SA3@CuMOFs groups, this may be because that NO release in both groups for the first 1 h is approximately the same according to the experimental results in Fig. 4b.
Dynamic coagulation test is another indicator to evaluate the hemocompatibility of the material. After incubating the samples with fresh blood for 20, 40 and 60 minutes, 2 mL PBS was added and the supernatant was transferred to detect absorbance at 545 nm. When it was coagulated and precipitated, the supernatant changed transparent and the absorbance decreased. The results were showed in Fig. 4c, the absorbance of supernatant in both NO@CuMOFs and NO@SA3@CuMOFs groups was significantly higher than that of the blank group, verifying that the NO loaded samples have an anticoagulant effect. Also, the anticoagulant capacity of NO@CuMOFs and NO@SA3@CuMOFs is no significant difference.
The minimum inhibitory concentration of NO@SA3@CuMOFs sample against Gram-negative E. coli and Gram-positive S. epidermidis was detected (ESI Fig. S2†). It is both 2.5 mg mL−1 for E. coli and S. epidermidis. Fig. 5 shows the inhibitory effect of the different nanoparticles on E. coli and S. epidermidis. CuMOFs without SA modification showed a weak antibacterial efficacy at the concentration of 2.5 mg mL−1. It can be seen that both NO loading groups had an significantly increased antibacterial function. The antibacterial rate of NO@SA3@CuMOFs against E. coli was about 90%, and the antibacterial rate of NO@CuMOFs against E. coli was above 95%. While both reached almost 100% against S. epidermidis. The antibacterial rate of NO@CuMOFs against E. coli was slightly higher than that of NO@SA3@CuMOFs, which may be because more initial Cu2+ release in this sample without SA modification.
Therefore, the results of this study indicate that the as synthesized NO-releasing CuMOFs have good anticoagulant and antibacterial activities, which are promising in application for blood contacting devices.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ra08066k |