Yingli
Shi
,
Chun Fang
Wen
,
Xuefeng
Wu
,
Jia Yue
Zhao
,
Fangxin
Mao
*,
Peng Fei
Liu
and
Hua Gui
Yang
*
Key Laboratory for Ultrafine Materials of Ministry of Education, Shanghai Engineering Research Center of Hierarchical Nanomaterials, School of Materials Science and Engineering, East China University of Science and Technology, 130 Meilong Road, Shanghai 200237, China. E-mail: hgyang@ecust.edu.cn; fxmao@ecust.edu.cn
First published on 4th March 2022
The electrochemical reduction reaction of CO2 provides a renewable method to close the carbon cycle and alleviate the global energy issue. Bi-based electrocatalysts present huge prospects for catalyzing formate-selective CO2 reduction. Herein, we fabricated a porous vegetable sponge-like bismuth oxide (VS-Bi2O3) for the selective electroreduction of CO2 to formate, which underwent in situ reconstruction to form 2D nanosheets containing metallic Bi and Bi2O2CO3. We propose that the unique porous morphology and low crystallinity of VS-Bi2O3 are beneficial for the in situ generation of Bi2O2CO3, which might play a significant role in enhancing the CO2 electrocatalysis performance. The catalyst delivers a 93.7% faradaic efficiency of formate at 400 mA cm−2 and shows stability for over 18 h at 100 mA cm−2.
O bond).4,10–14 A large reorganization energy in the first electron transfer step to form CO2˙− from CO2, −1.90 V versus the standard hydrogen electrode, imposes a high overpotential and a slow reaction rate.15 Furthermore, the hydrogen evolution reaction (HER) competes with the desired CO2RR, leading to a selectivity loss for the generation of formate.3,11 Therefore, developing efficient electrocatalysts with low overpotentials and high selectivity becomes a key challenge for exclusively reducing CO2 to formate.
Bismuth-based (Bi-based) materials, as efficient electrocatalysts, have aroused great interest in producing formic acid or formate from CO2, due to their low cost, low toxicity and environmentally benign traits.16–18 Due to the low carbon monoxide adsorption energy and strong stabilization of intermediates, Bi-based materials are thermodynamically favorable for yielding formate instead of competitive CO or H2.19,20 To implement the reaction, a high overpotential of over 300 mV must generally be applied along with a low current density (usually less than 100 mA cm−2, especially in H cell system).21,22 Structural engineering methods, such as morphology, component and defect engineering, have been reported to promote the catalytic activities of catalytic materials.23,24 Earlier studies regarding Bi-based catalysts with different morphologies, including dendrites, nanowires, nanoflakes, bismuthene nanosheets as well as nanoparticles, have been reported to deliver a high formate selectivity of over 90%.7,25 However, once they interact with the surrounding reactants or products under the reduction conditions, most of the catalysts are inclined to undergo structural self-reconstruction, which can change their morphology and structure, which thus further alters the activity and selectivity of the catalysts.22,26 For instance, Yao et al. proposed that the KHCO3 electrolyte could moderate the dissociation and conversion of the Bi-based metal–organic framework (Bi-MOF) into Bi2O2CO3, and the applied cathodic potential further helped to reduce the Bi2O2CO3 to metallic Bi, of which the unsaturated surface Bi atoms served as active sites.22 The work of Ma et al. reported bismuthene (Bi-ene) nanosheets derived from monoclinic scheelite BiVO4 under working conditions, which significantly enhanced the CO2 reduction performance.27 We anticipate that designing new precatalysts with specific structures will play a significant role in developing highly efficient Bi-based catalysts.
Bi2O3, which has both high physical and chemical stability, is convenient for synthesis reactions without being much affected by the surrounding environment. This can help to rule out unnecessary influences and focus on the research priorities. Besides, Bi2O3 possesses CO2RR advantages like other Bi-based materials. For example, the Bi–O structure of Bi2O3 has been reported to be conducive to CO2RR via enhancing the CO2 adsorption capacity and improving the stability of the CO2•− intermediate.28,29 Many Bi-based catalysts with the Bi–O structure, such as Bi2O3 nanosheet/nitrogen-doped graphene quantum dots (Bi2O3-NGQDs),30 β-Bi2O3 fractals31 and Bi2O3 nanosheets grown on a conductive multi-channel carbon matrix (Bi2O3NS@MCCM),32 exhibit a high CO2RR performance. Our aim is to prepare a highly active Bi2O3 material and study its in situ reconstruction process in electrolytic CO2 reduction.
Herein, a porous vegetable sponge-like bismuth oxide (VS-Bi2O3) was synthesized using a microwave ultrasonic synthesis method and exhibited an excellent performance for catalyzing CO2 to formate with a faradaic efficiency (FE) of around 93% under a potential ranging from −0.53 to −1.29 V (versus the reversible hydrogen electrode (RHE)), where all potentials are referenced to RHE unless mentioned otherwise) and a current density up to 400 mA cm−2 in the flow cell system. In situ reconstruction of VS-Bi2O3 took place under CO2RR conditions, with a fine nanosheet structure containing metallic Bi and Bi2O2CO3 formed. The porous structure of VS-Bi2O3 might be favorable for reconstruction during the CO2RR, and the generated Bi2O2CO3 could maintain the superior catalytic performance of formate generation, with scarce attenuation occurring under a current density of 100 mA cm−2 over 18 hours.
The produced VS-Bi2O3 was then calcined using a muffle furnace to fabricate the contrast bulk Bi2O3 (B-Bi2O3). The temperature was set as 500 °C and the furnace was supposed to reach that temperature in 100 minutes after which it remained at the same temperature for 1 h.
:
H2O = 3
:
1, v/v), followed by ultrasonication for 30 min to form an ink, which was then sprayed onto a piece of commercial Sigracet gas diffusion layer (GDS 28BC, Fuel Cell store), whose area was set as 3 × 3 cm2. After drying, a piece of 1.5 × 1.5 cm2 gas diffusion electrode (GDE) was tested using a flow cell reactor as the working electrode. The CO2 gas feed rate was set as 20 standard cubic centimeters per minute (sccm). The electrolyte was 1 M KOH, which flows at a rate of 10 mL per min. All potentials were calibrated to the reversible hydrogen electrode (RHE) with iRcell compensation (i serves as the applied current and Rcell denotes the cell resistance) according to the equation ERHE = EAg/AgCl + 0.205 + 0.059 × pH + i × Rcell. Gas products were analyzed via gas chromatography (RAMIN, GC2060), using a thermal conductivity detector (TCD) for detecting H2 and a flame ionization detector (FID) for the detection of CO and other gaseous hydrocarbons. The liquid product of HCOO− was quantified using 1H nuclear magnetic resonance (NMR). For analysis, 500 μL electrolyte with the liquid product in it was taken out to mix with 100 μL D2O (with TMSP as the internal standard) to form the mixture quantified later using NMR.
The scanning electron microscopy (SEM) images (Fig. 1b and c, and Fig. S1 and S2, ESI†) show a vegetable sponge-like morphology, assembling multiple pieces of nanosheets into a hierarchical micron structure. Transmission electron microscopy (TEM) results (Fig. 1d and e and Fig. S3, ESI†) show lots of open pores in the VS-Bi2O3. Moreover, the high-resolution TEM (HR-TEM; Fig. 1f) image displays no obvious lattice fringe. The selected area electron diffraction (SAED; inset in Fig. 1f) image exhibits a diffraction ring with a radius of 3.19 Å that corresponds to the (111) plane of Bi2O3 (PDF#27-0052), confirming the weak crystallinity of VS-Bi2O3. The B-Bi2O3 obtained from the VS-Bi2O3via annealing in air has a high crystallinity, with the XRD pattern aligning well with monoclinic Bi2O3 (PDF#41-1449) (Fig. S4, ESI†).
The CO2RR processes for VS-Bi2O3 and B-Bi2O3 were carried out in 1 M KOH electrolyte (pH = 14) using a flow cell system (Fig. S5, ESI†). During the CO2RR, VS-Bi2O3 underwent in situ reconstruction according to the XRD measurements for different electrolysis times. As shown in Fig. 2a, tetragonal Bi2O2CO3 (PDF#41-1488) appeared after 0.5 h of electrolysis at 100 mA cm−2. As the catalysis process proceeds, the featured peaks of Bi2O2CO3 (marked with purple stars) become noticeable for the XRD patterns after 3, 10, and 20 h. Furthermore, the Raman spectrum of the VS-Bi2O3 sample after electrolysis also demonstrates the formed Bi2O2CO3via the featured peaks appearing at 162 and 1069 cm−1 (in light orange shadow),22,34 while the peak at 95 cm−1 is attributed to Bi2O3 (in light grey shadow) (Fig. 2b).35 As for B-Bi2O3, scarce Bi2O2CO3 was detected after electrolysis (Fig. S6, ESI†).
To further analyse the surface valence states, X-ray photoelectron spectroscopy (XPS) was conducted. Post-electrolysis XPS inspections of VS-Bi2O3 (at 100 mA cm−2 for 24 h) are shown in Fig. 2c–e. The peaks at 159 and 164.3 eV in the Bi 4f spectrum (Fig. 2c) are assigned to Bi3+, demonstrating a single oxidation state of Bi3+.28,30 Three obvious fitted peaks can be clearly identified in the O 1s spectrum (Fig. 2d). The peaks at 529.6, 530.7 and 531.5 eV correspond to the O atoms in the Bi–O bonds in the [Bi2O2]2+ layers, the O atoms in C–O in the [CO3]2− layers, and the oxygen of adsorbed O2, respectively.7,28,34 As for the C 1s XPS spectrum (Fig. 2e), the peak at 289.0 eV is indexed to the carbon atoms in the [CO3]2− layers.36 XPS spectroscopy verifies the existence of Bi2O2CO3 after electroreduction, in line with the XRD and Raman results.
To gain further insight into the morphology changes, SEM, TEM and HR-TEM characterizations of the post-electrolysis sample of VS-Bi2O3 were carried out. As shown in Fig. 3a and b, vegetable sponge-like frames of VS-Bi2O3 evolve into a nanosheet morphology after CO2RR for 10 h. Combined with more post-electrolysis SEM images for different timescales in Fig. S7 and S8 (ESI†), we speculate that the morphology of VS-Bi2O3 underwent several transformation steps under different cathodic potentials. The shape first transformed from the vegetable sponge-like to thick nanosheet-assembled plates, and then gradually changed into thin nanosheets. The TEM image (Fig. 3c) confirms the nanosheet morphology in accordance with the SEM images. The SEM images after electrolysis of B-Bi2O3 are also displayed in Fig. S9 and S10 (ESI†). Scanning transmission electron microscopy-energy dispersive spectroscopy (STEM-EDS; Fig. 3d) shows the uniformly distributed Bi, O and C elements. It is worth noting that the presence of the carbon element to some extent reveals the existence of Bi2O2CO3. The high-resolution TEM image in Fig. 3e proves this point as well, with the lattice spacing of 2.95 Å aligning well with the (013) facet of Bi2O2CO3. Fig. 3f shows a 3.28 Å lattice space in accordance with the (012) plane of metallic bismuth, which was derived from the in situ reduction of VS-Bi2O3.
The above measurements illustrate that the prepared VS-Bi2O3 is prone to undergo reconstruction under the working conditions. The sample was changed into metallic bismuth and Bi2O2CO3 after electrolysis, among which the Bi2O2CO3 did not appear in the B-Bi2O3 sample (Fig. S6, ESI†). Besides, the porous vegetable sponge-like morphology is inclined to be exposed to the operating environment since its open pores can be filled with electrolytes and reactants. This may lead to the reconstruction from VS-Bi2O3 to Bi and Bi2O2CO3 during the CO2RR process. Bi2O2CO3 is a layered structure consisting of CO32− and [Bi2O2]2+, which has been reported to exhibit a lower overpotential compared with metallic bismuth.37
To figure out the phase transformation from Bi2O3 to Bi2O2CO3 and Bi, three XRD samples obtained under different conditions were prepared (Table S1 and Fig. S11, ESI†). The results indicate that VS-Bi2O3 did not react directly with the KOH electrolyte in the absence of CO2 under ambient conditions. However, when VS-Bi2O3 was introduced into the CO2 atmosphere, Bi2O2CO3 was generated with no metallic Bi formed. Furthermore, the VS-Bi2O3 changed into metallic Bi and Bi2O2CO3 with the current density applied. Based on the above results, we speculated that the Bi2O2CO3 might be formed via the intercalation of CO32− into the layered structure of the bismuth oxide compound. Previous reports have revealed that the presence of CO2 during the CO2RR process plays a significant role in maintaining the stable existence of Bi2O2CO3 thanks to the consumption of most cathodic electrons.37,38 Besides, a high local pH was also reported to be beneficial for the formation of Bi2O2CO3, and the 1 M KOH electrolyte in this work can provide a large amount of OH−, which might promote the generation of Bi2O2CO3.7
We then carried out the CO2RR to assess the electrocatalytic performance and identify the role of Bi2O2CO3. As shown in Fig. 4a and Fig. S12 (ESI†), VS-Bi2O3 achieves a high current density of up to 100 mA cm−2 at a small applied potential of only −0.53 V, with an accompanying high FE(HCOO−) of around 93.6%. The FE(HCOO−) remains at a high level of >93.0% over a wide potential range from −0.53 V to −1.29 V, with a potential window of 760 mV. The maximum FE(HCOO−) of 94.9% appears at −1.12 V delivering a current density of 300 mA cm−2. The overall current density of 400 mA cm−2 is achieved at a potential of −1.29 V, in the meantime sustaining a high FE(HCOO−) of around 93.7%. As for the contrast sample, B-Bi2O3 attains the same current density with a much more negative potential and a much lower selectivity for formate. Taking the current density of 200 mA cm−2, for example, B-Bi2O3 needs an applied potential of −1.11 V to reach that goal, which is 380 mV more negative than VS-Bi2O3 with a low FE(HCOO−) of 85.3% under the operational conditions (Fig. 4b, and Fig. S13, ESI†). Furthermore, the potential grows markedly for the larger current densities, and a potential of −1.58 V is needed for 400 mA cm−2, negatively shifted by 300 mV compared with VS-Bi2O3. The CO2RR performance measurements unveil the superb activity and exclusive selectivity of VS-Bi2O3 for the electrochemical conversion of CO2 into formate, indicating the significance of Bi2O2CO3 derived from VS-Bi2O3.
Since efficient charge transfer at the catalyst/electrolyte interface is beneficial to the catalytic process, we carried out electrochemical impedance spectroscopy (EIS) in order to measure the kinetics of charge transfer.35Fig. 4c shows the Nyquist plots of VS-Bi2O3 and B-Bi2O3 under open-circuit potential at a steady state, from which a smaller arc can be observed in VS-Bi2O3 (red) compared with B-Bi2O3 (blue). In the Nyquist plots, the charge transfer resistance (Rct) of the electrochemical reaction can be represented by the radius of the arc, and a smaller arc usually means a smaller resistance. Thus, VS-Bi2O3 possesses a highly accelerated charge-transfer process thanks to its much shorter radius than the contrast bulk sample. We attributed this remarkable improvement to the appearance of Bi2O2CO3 derived from VS-Bi2O3. Hence durability testing was carried out at the current density of 100 mA cm−2, and the potential remained steady without any significant degradation for an electrolysis process of over 18 h, demonstrating its superior stability for converting CO2 to formate (Fig. 4d). The performance comparison of VS-Bi2O3 with previous Bi-based materials is listed in Table S2 (ESI†).
Bi2O2CO3 is a layered structure consisting of CO32− and [Bi2O2]2+.37 The presence of metastable oxides has previously been reported to be able to stabilize the reduced CO2 intermediate, which plays a vital role in lowering the overpotential and accelerating the charge transfer required to reduce CO2 into the target formate product.7,37–39 The Bi2O2CO3 was generated in situ from VS-Bi2O3 during the CO2RR process, whose existence after electrolysis at 100 mA cm−2 for 20 h revealed that the formed Bi2O2CO3 was robust enough to survive under an applied cathodic bias. However, the contrast sample B-Bi2O3 was reduced in situ to metallic Bi without Bi2O2CO3 and was accompanied by an unsatisfactory performance. Therefore, the presence of Bi2O2CO3 might play a significant role in enhancement of the CO2RR performance.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: 10.1039/d1qm01557e |
| This journal is © the Partner Organisations 2022 |