Niklas
Stegmann
,
Hilke
Petersen
,
Claudia
Weidenthaler
and
Wolfgang
Schmidt
*
Department of Heterogeneous Catalysis, Max-Planck-Institut für Kohlenforschung, Kaiser-Wilhelm-Platz 1, D-45470 Mülheim an der Ruhr, Germany. E-mail: schmidt@mpi-muelheim.mpg.de
First published on 18th August 2021
Novel and known low-valent transition metal phosphates (TMPs) are accessible via a novel and facile pathway. The method allows syntheses of TMPs also with reduced oxidation states. The key feature of the new route is the reductive character of a hypophosphite salt melt, which acts as reaction medium and enables directing the oxidation state of the transition metal.
Synthetic phosphate salts are known for most transition metals. Considering the number of metal cations and the structural variety of condensed phosphate units, the sheer quantity of different phases is staggering. The variety of compounds formed by the class of TMP materials is primarily limited by the intrinsic chemical nature of the elementary ionic building units. However, it can be also restricted by availability of precursors and preparation methods. In literature, versatile preparation methods, such as hydrothermal procedures, molten salt processes, or simple precipitation, are established for the synthesis of highly crystalline bulk TMPs. Application of TMPs as functional materials often requires quite sophisticated preparation methods though. Structure directing techniques are used to optimize the performance of the materials, porosity is generated via nanocasting strategies, thin films are formed via gas phase deposition, and nanoparticles are synthesized by electrochemical approaches.12,14–18 No matter what kind of technique is used or what kind of application is envisaged, all methods have in common the use of phosphate-based precursor compounds, very different to the method presented here. In contrast to conventional syntheses, in our route a hypophosphite salt acts as precursor in combination with metal oxides. While the molten hypophosphite salt serves concurrently as reaction medium and phosphate precursor, the metal oxide provides the transition metal cation under reductive conditions. Due to the reducing character of the hypophosphite melt, the transition metal gets reduced during the TMP formation.
The molten salt method is thus a simple and versatile approach, which can be used for the synthesis of known and novel first row transition metal phosphates with low oxidation states at moderate temperatures (300–500 °C). This approach was tested for a series of first row transition metals (Ti, V, Cr, Mn, Fe) under low (300 °C) and high (500 °C) temperature conditions. The results, listed in Table 1, indicate that low temperature conditions tend to form ammonium TMPs, while higher temperatures lead to the formation of ammonium-free TMPs with condensed metaphosphate structures. In almost all cases, the reaction was accompanied by a reduction of the transition metal.
Precursor | Product (300 °C) | Product (500 °C) | |||
---|---|---|---|---|---|
TM oxide | o. s | TMP | o. s | TMP | o. s |
TiO2 | 4+ | Ti(III)p | 3+ | Ti(PO3)3 | 3+ |
V2O5 | 5+ | V(PO3)3 | 3+ | V(PO3)3 | 3+ |
Cr2O3 | 3+ | Cr(NH4)HP3O10 | 3+ | Cr2(P6O18) | 3+ |
MnO2 | 4+ | — | — | Mn2(P4O12) | 2+ |
Fe2O3 | 3+ | Fe(II)p | 2+ | Fe2(P4O12) | 2+ |
In a typical reaction, a metal oxide powder, such as TiO2, V2O5, Cr2O3, MnO2, or Fe2O3, is mixed with a surplus of hypophosphite (NH4H2PO2) and heated briefly in a tube furnace under inert gas flow. Then the melt is cooled down and washed with water to yield the pure TMPs (Fig. S1 in ESI†). Detailed synthesis parameters for a series of transition metal compounds are reported in the ESI.† The process window of the method is determined by the temperature and time between the melting point and the thermal decomposition of the hypophosphite precursor (Fig. S2†). The hypophosphite melt mediates the reaction with the dispersed or dissolved metal oxides.
Due to the thermodynamic instability of the hypophosphite anion, the disproportionation into phosphane gas and phosphates limits the reaction. The phosphane acts as spectator under the presented reaction conditions. Excess phosphate compounds, as formed on the crystal surfaces, can easily be removed by washing with water. Formation of metal phosphides via reaction of phosphane and metal oxides, as often described in literature, was not observed under the reaction conditions used here.
A representative example is the reaction of titanium(IV) oxide (P25) and ammonium hypophosphite, resulting in novel and known crystalline titanium(III) phosphate compounds. At 300 °C an unknown crystalline ammonium titanium(III) phosphate compound (NH4Ti(III)P2O7), denoted as Ti(III)p, is formed from the melt as illustrated by the respective XRD pattern in Fig. 1a and S3.† The product is a pyrophosphate as evidenced by a characteristic band at 764 cm−1 in its Raman spectrum. Increasing the reaction temperature to 500 °C yields a known titanium(III) trimetaphosphate, Ti(PO3)3 (Fig. 1c). In this structure the isolated TiO6 octahedra are linked through infinite chains of PO4 tetrahedra.19
The formation of a melt by using an excess of hypophosphite is indispensable for complete conversion of the TiO2 and high crystallinity of the product. Syntheses of Ti(PO3)3 with increasing weight ratios of hypophosphite precursor result in different phase compositions as documented by the XRD patterns in Fig. 2. Lower ratios of the hypophosphite precursor (1/1–1/2) are apparently not sufficient to convert the TiO2 quantitatively. However, also these conditions cause partial reduction and the formation of stable titanium(III) oxide species on the surfaces of the titania particles as indicated by the characteristic black coloration and confirmed by XPS spectra (Fig. 3d). Unknown intermediate phases are formed by increasing hypophosphite ratios (1/3–1/5 in Fig. 2) before phase pure Ti(PO3)3 is obtained from the melt (ratio ≥1/6 in Fig. 2).
![]() | ||
Fig. 3 XPS spectra of (a) Ti(III)p, (b) Ti(PO3)3, (c) Ti(IV)p and (d) reductively phosphated Ti(III/IV) oxide synthesized from a mixture of TiO2 and NH4H2PO2 with a weight ratio of 1/2. |
In a proposed redox reaction mechanism, the precursors can be considered as oxygen donor and acceptor pairs. While the hypophosphite acts as oxygen acceptor to form stable phosphate compounds, the metal oxide donates oxygen atoms under reductive conditions. Provided that sufficient hypophosphite is available, all oxygen of the metal oxide will be consumed and the reduced cations are free to form crystalline TMP phases. Reports on low-valent titanium(III) phosphates are rather rare in literature, likely due to their strong tendency to oxidize in air.20 XPS spectra show the presence of two different titanium species on the crystal surfaces of Ti(III)p and Ti(PO3)3 as shown in Fig. 3a and b. They can be attributed to Ti(III) and Ti(IV) indicating that the Ti(IV) species exist on the crystal surface in both compounds, likely as the result of oxidation of Ti(III) on the surface by ambient air. XPS analysis probes surface-near regions of the particles, thus, the Ti(IV) signal is caused by surface species. Crystalline Ti(PO3)3 is known to be a pure Ti(III) compound.19
The bulk of the novel Ti(III)p compound offers a good thermal and chemical stability as indicated by XRD data. It is longtime-stable in acidic aqueous solution even at elevated temperature (H3PO4, pH = 1, 80 °C, 72 h) and also thermally stable in ambient air up to 250 °C. At higher temperature in air, the material undergoes a phase transformation to a known titanium(IV) pyrophosphate (TiP2O7). Under non-oxidative conditions, thermal treatment of Ti(III)p yields another novel crystalline Ti(IV) phosphate (Ti(IV)P2O7), denoted as Ti(IV)p, showing exclusively Ti(IV) species (Fig. 3c). TG/DSC-MS (Fig. S4 and S5†) reveals that the phase transformation is accompanied by release of ammonia, hydrogen, and water. The XRD pattern of the novel Ti(IV)p is presented in Fig. 1b and S6.† Reproducibility and purity of the novel crystalline diamagnetic Ti(IV)p compound was confirmed by 31P MAS NMR spectra (Fig. S7†) showing no additional crystalline phase or any amorphous phase in the product (see ESI,† for details). SEM images show a homogenous distribution of micrometer sized crystals for pristine Ti(III)p and Ti(IV)p (Fig. S8†).
Overall, the conversion of TiO2 with ammonium hypophosphite offers reaction pathways to several known titanium phosphate compounds as well as two novel phases as sketched in Fig. 4. As representative example, the reductive phosphatization of Ti(IV) to Ti(III) shows the reductive feature and variability of the hypophosphite route.
![]() | ||
Fig. 4 Reaction pathways for the preparation of novel and known titanium phosphate phases accessible by reductive phosphatization of TiO2 in a melt of ammonium hypophosphite. |
Formation of low-valent TMPs, as reported here for the titanium compounds, is observed also for other transition metal compounds. Via identical synthesis procedures V(PO3)3, Cr(NH4)HP3O10, Cr2(P6O18), Mn2(P4O12), Fe(II)p (new phase), and Fe2(P4O12) were readily obtained (see ESI,† for details). In literature, low oxidation states of TMPs are generally reported to be accessible by using metal powders or low-valent metal compounds as precursors. In comparison, the new route offers the possibility to direct the oxidation state of the transition metal via the hypophosphite, which results in quite moderate reaction conditions.
In summary, first-row transition metal oxides are converted in a hypophosphite melt to crystalline metal phosphates. The facile method operates at moderate temperatures (300–500 °C) and offers access to a number of novel, known and, very specifically, low-valent TMPs. The reducing feature of the hypophosphite precursor is exemplified by the reaction with TiO2 resulting in a number of known and novel Ti(III) and Ti(IV) phosphates. Reaction of the hypophosphite with other transition metal oxides (Cr, V, Mn, Fe) revealed comparable results, i.e., formation of transition metal phosphates with reduced and stabilized oxidation states of the metal cation. Overall, the synthesis of transition metal phosphates via a hypophosphite melt provides a highly versatile route towards products with rich structural and compositional variety for a class of materials that is key for various future technologies, including energy storage, power generation, catalysis and optical applications.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ta03782j |
This journal is © The Royal Society of Chemistry 2021 |