Open Access Article
Qiang
Fu
*a,
Jiaqi
Wang
a,
Angelina
Sarapulova
a,
Lihua
Zhu
a,
Alexander
Missyul
c,
Edmund
Welter
d,
Xianlin
Luo
a,
Ziming
Ding
ef,
Michael
Knapp
a,
Helmut
Ehrenberg
ab and
Sonia
Dsoke
ab
aInstitute for Applied Materials (IAM), Karlsruhe Institute of Technology (KIT), Hermann-von-Helmholtz-Platz 1, D-76344 Eggenstein-Leopoldshafen, Germany. E-mail: qiang.fu@kit.edu; Fax: +49-721 608-28521; Tel: +49-721 608-41445
bHelmholtz Institute Ulm for Electrochemical Energy Storage (HIU), Helmholtzstrasse 11, 89081 Ulm, Germany
cCELLS-ALBA Synchrotron, E-08290 Cerdanyola del Valles, Barcelona, Spain
dDeutsches Elektronen-Synchrotron DESY, Notkestraße 85, D-22607 Hamburg, Germany
eInstitute of Nanotechnology (INT), Karlsruhe Institute of Technology (KIT), Hermann-von-Helmholtz-Platz 1, D-76344 Eggenstein-Leopoldshafen, Germany
fTechnische Universität Darmstadt, 64289 Darmstadt, Germany
First published on 27th July 2021
The electrochemical performance and reaction mechanism of orthorhombic V2O5 in 1 M ZnSO4 aqueous electrolyte are investigated. V2O5 nanowires exhibit an initial discharge and charge capacity of 277 and 432 mA h g−1, respectively, at a current density of 50 mA g−1. The material undergoes quick capacity fading during cycling under both low (50 mA g−1) and high (200 mA g−1) currents. V2O5 can deliver a higher discharge capacity at 200 mA g−1 than that at 50 mA g−1 after 10 cycles, which could be attributed to a different type of activation process under both current densities and distinct degrees of side reactions (parasitic reactions). Cyclic voltammetry shows several successive redox peaks during Zn ion insertion and deinsertion. In operando synchrotron diffraction reveals that V2O5 undergoes a solid solution and two-phase reaction during the 1st cycle, accompanied by the formation/decomposition of byproducts Zn3(OH)2V2O7·2(H2O) and ZnSO4Zn3(OH)6·5H2O. In the 2nd insertion process, V2O5 goes through the same two-phase reaction as that in the 1st cycle, with the formation of the byproduct ZnSO4Zn3(OH)6·5H2O. The reduction/oxidation of vanadium is confirmed by in operando X-ray absorption spectroscopy. Furthermore, Raman, TEM, and X-ray photoelectron spectroscopy (XPS) confirm the byproduct formation and the reversible Zn ion insertion/deinsertion in the V2O5.
Many efforts have been made on the exploration of high-performance positive electrode materials for ARZBs, including the polymorphs of manganese oxide (α-, β-, γ-, δ-MnO2, and spinel-MnO2),4,6–17 Prussian blue analogues,18–21 vanadium-based oxides (Ca0.25V2O5·nH2O, Zn0.25V2O5·nH2O, Na0.33V2O5, V2O5·nH2O, LiV3O8, and H2V3O8),2,5,22–38 organic compounds,39,40 and other compounds such as Na3V2(PO4)3,41 Na3V2(PO4)2F3,42 VS2,43 and Mo6S8.44 Among them, vanadium-based oxides are very promising due to their open framework and relatively high capacity as well as operation voltage of around 0.6–1.0 V. For example, Kundu et al.5 reported Zn0.25V2O5·nH2O positive electrode, which delivers a high initial discharge/charge capacity of 282/278 mA h g−1 at C/6 rate, excellent rate capability, and high cycling stability with a capacity retention of 80% after 1000 cycles at 15C rate. Xia et al.29 demonstrated that Na0.33V2O5 nanowires have a high capacity of 367.1 mA h g−1 at 100 mA g−1 when used as the positive electrode in ARZBs. This material also exhibits good rate capability and high capacity retention of 93% after 1000 cycles. Pang et al.34 investigated H2V3O8/graphene composite, which shows a high capacity of 394 mA h g−1 at C/3, high rate capability, and excellent cycling stability with a capacity retention of 87% after 2000 cycles. Despite this significant progress, it is still urgently required to deeply understand the electrochemical reaction mechanism of positive electrode materials. Because it is more meaningful to the development of ARZBs by understanding the reaction mechanism behind good electrochemical performance than trying to improve performance empirically.
Because of its typical layered structure and relatively high capacity, V2O5 is considered a promising positive electrode for ARZBs.45–48 Despite its good electrochemical performance in ARZBs, the structural changes of V2O5 during electrochemical processes are still under debate. Three different viewpoints regarding the structural changes of V2O5 in ARZBs have been proposed so far:
(i) Zhou et al.46 compared the performance of V2O5 in different electrolytes (i.e. Zn(NO3)2, Zn(CH3COO)2, ZnCl2, and ZnSO4 aqueous-based electrolytes) and with different concentrations of ZnSO4-based electrolytes. In 3 M ZnSO4, V2O5 delivers the best performance with a high capacity of 224 mA h g−1 at 100 mA g−1 and good cycling stability at the high current densities of 1 and 2 A g−1, respectively. Ex situ X-ray diffraction (XRD) demonstrated the formation of a new phase of ZnxV2O5 upon Zn insertion into V2O5.
(ii) Zhang et al.45 also reported a V2O5 cathode material with a capacity of 470 mA h g−1 at 0.2 A g−1 and high capacity retention of 91.1% after 4000 cycles at 5 A g−1 in 3 M Zn(CF3SO3)2 electrolyte. They proved that this material can work in extreme conditions at both high (50 °C) and low (−10 °C) temperatures. The co-insertion of hydrated Zn ions into the V2O5 crystal structure was proposed based on ex situ XRD, X-ray photoelectron spectroscopy (XPS), and transmission electron microscopy (TEM).
(iii) Chen et al.47 proposed a phase transition reaction mechanism via ex situ XRD, Raman, and XPS. Orthorhombic V2O5 underwent a phase transition to zinc pyrovanadate during the first discharge, where the formed zinc pyrovanadate showed reversible Zn2+ (de)insertion during subsequent cycles.
However, the electrochemical reaction mechanism of V2O5 in the above-reported works was investigated through ex situ techniques. The findings are in controversy with each other and a detailed investigation of the structural changes of V2O5 upon Zn-ion insertion/deinsertion is still missing. Moreover, non-equilibrium or intermediate species or states cannot be detected using ex situ studies, while in operando studies can provide a more reliable understanding of the structural evolution of a battery material in “real use”.
In addition, it has been frequently reported that a mass of complex byproducts was produced/decomposed during the discharge/charge cycling of vanadium oxides such as NaV3O8·1.5H2O,2 VO1.52(OH)0.77,24 Zn2V2O7,35 and NH4V4O10.49 Interestingly, byproducts were not observed in the three works related to the study of V2O5 reported above. To better understand the electrochemical mechanism of V2O5 in ARZBs in operando techniques like diffraction using synchrotron radiation are required. Due to their extremely bright, high flux, and tunable also high energy, synchrotron radiation-based characterization provides deep penetration into the sample, high-quality data, and real-time diffraction. Particularly, in operando synchrotron study can effectively avoid the unpredictable contamination and irreversible changes of highly reactive samples during material preparation, handling, and transportation, which can provide more reliable and precise data for analysis. Hence, in this work, orthorhombic V2O5 were prepared by a facile hydrothermal method and the detailed structure evolution and reaction mechanism of orthorhombic V2O5 in ARZBs are studied via in operando synchrotron diffraction and X-ray absorption spectroscopy (XAS) together with ex situ Raman, TEM, and X-ray photoelectron spectroscopy (XPS).
:
20
:
10 with N-methyl-2-pyrrolidone solvent. The dried electrode mixture with mass loading of ∼1.4 mg cm−2 was pressed (4 tons) on a stainless steel mesh of 12 mm and dried at 120 °C overnight under vacuum. CR2032-type coin cells for electrochemical measurements were assembled in air at room temperature. The cells were built with V2O5 positive electrode, Zn foil as the negative electrode, 1 M ZnSO4 as the electrolyte, and a piece of glass microfiber (Whatman) as the separator. The galvanostatic cycling with the potential limitation (GCPL) and cyclic voltammetry (CV) measurements were performed between 0.3 and 1.6 V (vs. Zn2+/Zn) with a VMP3 potentiostat (BioLogic) at 25 °C. GCPL was performed at different current densities ranging from 50 to 1600 mA g−1 to determine the rate capability of the battery.
![]() | ||
| Fig. 1 Rietveld refinement based on synchrotron diffraction data (a), SEM (b), and HRTEM image (c) of V2O5 nanowires, where Fast Fourier Transform (FFT) was done from the marked orange area. | ||
To investigate the structural evolution of V2O5 upon Zn-ion insertion/deinsertion, in operando synchrotron diffraction was performed during the initial 1.5 cycles. The contour maps of selected diffraction patterns and corresponding voltage–time profiles are provided in Fig. 4. Note that an electrochemical activation is observed at the high current of 200 mA g−1 during the first 5 cycles, with very interesting changes. Here we go deeper on understanding the very initial changes at low current and in the future, it would be interesting and necessary to study what is happening during the further cycles at higher current density.
![]() | ||
| Fig. 4 Contour maps of in operando synchrotron diffraction of V2O5 during the first one and half cycles and the corresponding voltage profile at a current density of 50 mA g−1. | ||
Before the discharge (at 1.2 V), all reflections of the parent material can be indexed on the orthorhombic V2O5 in the space group Pmn21 (see Fig. S2a† for the Rietveld refinement of pristine V2O5). At the beginning of the 1st discharge (Region I), most of the characteristic reflections of V2O5, such as ones at 200 (4.12°), 101 (6.96°), 400 (8.24°), 011 (8.58°), 301 (9.08°), 411 (11.90°), 600 (12.37°), 002 (13.31°), 012 (14.38°), 402 (15.67°), and 701(15.91°), continuously shift towards lower 2θ, accompanied by a slight reduction of their intensity. Therefore, a solid solution reaction upon Zn ions insertion into the V2O5 structure can be proposed up to the stoichiometry ZnxV2O5 (x = 0.22, 65 mA h g−1, black line at the end of Region I, Fig. S3†), where lattice parameters a and c increase and b decreases. At the same time, few reflections at 010 (5.42°), 020 (10.85°), and 120 (11.04°) slightly shift to high angles; few other reflections at 110 (5.80°), 320 (12.49°), 021 (12.73°), and 620 (16.46°) keep in the same positions. Upon total discharge capacity of 44 mA h g−1 from OCV (1.02 V, x = 0.15, cyan line in the middle of Region I, Fig. S3†), two small reflections at 3.29° and 13.23° emerge, which belong to a new phase of zinc pyrovanadate of 1.2%(wt/wt), Zn3+δ(OH)2V2O7·2H2O (see Fig. S2b† for the Rietveld refinement based on the 10th pattern recorded during discharge of V2O5). Other reflections related to this phase become visible at 4.49°, 7.78°, 7.99°, 8.46°, 9.57°, 10.20°, 11.16°, 15.97°, and 17.54° along with further Zn ions insertion. At the same time, other reflections at 3.81°, 5.67°, 7.01°, 7.61°, 11.42°, and 11.66° appear and grow (Region II). These reflections are attributed to the formation of the new Zn-rich phase ZnxV2O5 (x = 0.44) through a 2-phase reaction, corresponding to the capacity of 129 mA h g−1. Meanwhile, the reflections of the new Zn-rich phase Zn0.44V2O5 remain in their positions, together with the decrease of the intensities of the Zn0.22V2O5 phase. At the end of Region II (gray line in Fig. S3†), most of the reflections of Zn0.22V2O5 phase disappear, and the Zn-rich Zn0.44V2O5 phase grows up. It implies the 2-phase coexistence transition between Zn0.22V2O5 and Zn0.44V2O5 in Region II during the Zn ions insertion. The formation of Zn0.44V2O5 is accompanied by the formation of the byproduct Zn3(OH)2V2O7·2H2O. Note that the x value is determined without the consideration of the consumption of V2O5 to form the byproduct Zn3+δ(OH)2V2O7·2H2O and the possible dissolution of V2O5, where the dissolution and phase transformation mechanisms of V2O5 in ARZBs were newly reported.58 Therefore, the value of x = 0.44 is an estimate for the lower limit of the inserted Zn content. Upon further Zn ions insertion (Region III), some new reflections begin to appear at 2.16°, 4.34°, 9.26°, 9.35°, which are assigned to the byproduct of ZnSO4Zn3(OH)6·5H2O with space group P
. Once the byproduct is formed, all its Bragg reflections remain at the same 2θ-positions throughout the discharge process, but their intensities increase. Meanwhile, most of the reflections maintain their positions along with the increase of their intensities (Region III), while only two reflections of Zn0.44V2O5 at 3.81° and 7.01° shift to high and low angles, respectively. It indicates that a solid solution process happens in Region III to form a final phase Zn0.94V2O5 together with the above-mentioned two byproducts with a total discharge capacity of 277 mA h g−1 (see Fig. S2c† for the Rietveld refinement of 36th pattern at first fully discharged V2O5). During the 1st charge, the reflections do not evolve in a symmetric reverse backway, as indicated by the appearance and disappearance of a small reflection at 7.17°, where two 2-phase regions are observed (Region II). The reflections return back to their initial 2θ-positions for the pristine V2O5 state, but with much lower intensities (see Fig. S2d† for the Rietveld refinement, based on the 69th pattern at fully charged V2O5). This is possibly caused by the amorphization of the crystalline active material or by the vanadium dissolution in the electrolyte32,36 (see Fig. S4†). Interestingly, both byproducts disappear again along with the 1st charging process. The evolution of the reflections in the 2nd discharge is analogous to that during the 1st cycle. In Region I, the reflections show the same behavior as those for the first discharge process, suggesting a solid solution reaction. In Region II and III, the electrode undergoes the same process: a shorter two-phase transition and solid solution than in the first discharge, but without the appearance of the reflections related to the byproduct Zn3+δ(OH)2V2O7·2H2O (see Fig. S2e† for the Rietveld refinement, based on the 97th pattern at the 2nd fully discharged V2O5). The formation of the other byproduct ZnSO4Zn3(OH)6·5H2O is also detected again during the second discharge process. The Zn3+δ(OH)2V2O7·2H2O has an open layered structure and has been reported by Alshareef et al.26 as positive electrode material in ARZBs. The material has a capacity of 213 mA h g−1 at 50 mA g−1 and shows a shift of the reflection 001 during Zn-ion insertion and deinsertion.26 This means that the Zn3+δ(OH)2V2O7·2H2O byproduct, generated during cycling, still contributes to the overall capacity of the electrode. Recently, Chen et al.47 reported that Zn3(OH)2V2O7·2H2O is also formed via the 2-phase coexistence transition in an aqueous Zn–V2O5 battery, and then it functions as a host structure in the following cycles, where it shows a shift of reflection 001 during Zn ion insertion. However, in our case, the shift of the 001 reflection is not observed, which might suggest that Zn3+δ(OH)2V2O7·2H2O is not active or just the c-axis parameter does not change. Furthermore, our results directly show for the first time the formation and decomposition of both byproducts Zn3+δ(OH)2V2O7·2H2O and ZnSO4Zn3(OH)6·5H2O during cycling.
In order to investigate the variation of the oxidation state and the local electron environment of vanadium during the discharge/charge (i.e. Zn insertion/deinsertion) process, in operando XAS was performed on the V2O5 nanowires as positive electrode within an in operando coin cell. Fig. 5 shows the normalized V K-edge spectra collected during the initial discharging and charging processes and reference spectra of standard vanadium oxides, where V2O5, VO2, and V2O3 have the oxidation state of +5, +4, and +3, respectively. The edge position of the V K-edge in the pristine V2O5 positive electrode overlaps with that of the standard V2O5 reference, indicating that the oxidation state of V in V2O5 is +5. Moreover, an intense pre-edge peak for the V K-edge of pristine V2O5 is observed, which is ascribed to the transitions between the 1s and bound p-hybridized d-states.59,60 Along with progressive discharging, the main absorption edge shifts towards lower binding energies, confirming the reduction of the oxidation state of vanadium upon the Zn-ion insertion. Meanwhile, the pre-peak (A in Fig. 5a) also shifts gradually to lower binding energy with the simultaneous decrease of intensity, confirming the reduction of V and the deformation of the local V environments during Zn-ion insertion. This is due to the co-existence of a distorted tetragonal pyramid and VO6 octahedra. The edge resonance (B in Fig. 5a) displays distinct changes in both intensity and shape, which is caused by the absorption of photons accompanied by core-electron excitations.60,61 During the discharge process, two broad peaks centered at 5494 eV and 5507 eV shift to lower energy and with a decrease of their intensities, before they converge into one very broad peak centered at 5500 eV from the initial stage to 0.99 V (peak B in Fig. 5a). After that, the formed broad peak centered at 5500 eV and the peak at 5486.5 eV continuously shift to lower energy accompanied by an increases of both intensities (from 0.99 V to 0.3 V). Two distinct isosbestic points62 at ∼5474 eV and ∼5502 eV (red arrows in Fig. 5a and b) are observed during both discharge (from 0.99 V to 0.3 V) and charge (from 0.3 V to 1.32 V) processes. This confirms the 2-phase coexistence transitions upon Zn-ion insertion/deinsertion into/from V2O5 structure, as already proposed from in operando synchrotron diffraction. At the fully discharged state at 0.30 V, the observed energy of the V K-edge lies almost in the middle of those of the V2O5 and V2O3 reference spectra. This means that the oxidation state of V is very close to V4+, in good agreement with the electrochemical data (see Fig. S5†). However, the energy of the edge does not completely overlap with the spectrum of VO2, reflecting structural differences between the discharged state with x = 1.00 in ZnxV2O5 and the reference material VO2. During the charging process (Zn-ion deinsertion), a completely reversible behavior can be observed. Pre-peak and edge resonance (A′ and B′ in Fig. 5a and b) prove a reversible process. At the fully charged state of ∼1.6 V, the V spectrum returns back to its initial state, indicating that the V ions are fully oxidized to the oxidation state of +5. The evolution of V K-edge spectra reveals that the V ions are reduced and reversibly oxidized during the Zn-ion insertion and deinsertion, respectively, accompanied by the local structural changes around the V ions and in full agreement with in operando synchrotron diffraction.
![]() | ||
| Fig. 5 In operando V K-edge XANES spectra during the 1st discharge (a) and charge (b) in 1 M ZnSO4; the isosbestic points are pointed out by red arrows. | ||
Raman spectra were collected to investigate vibration modes as fingerprints of the short-range structure of the samples during Zn-ion insertion/deinsertion, as displayed in Fig. 6 and Table S1.† In the pristine V2O5, oxygen atoms lie in four distinct sites in a [VO5] pyramid unit, denoted as O(1)–O(4). The stretching mode of V–O(1) bond is located at 994 cm−1 and its bending vibrations are located at 405 and 284 cm−1. Raman peaks at 482 cm−1 and 701 cm−1 are ascribed to the bending vibration of the V–O(3) and the stretching vibration of the V–O(2), respectively. The peaks at 527 and 304 cm−1 are attributed to the stretching and bending vibrations of the V–O(4) bond, respectively. The peaks at lower wavenumbers, 145 and 197 cm−1 are assigned to weak van der Waals interaction between adjacent [VO5] slabs. These results are consistent with previous works.63,64 After Zn-ion insertion, significant changes are observed and some peaks related to V2O5 at 994, 701, 405, 304, and 284 cm−1 become weak and broad, while those at 527, 482, and 197 cm−1 completely disappear. Meanwhile, some broad and distinct new peaks appear at 1129, 967, 876, 610, and 450 cm−1 for discharged V2O5, where peaks at 1129, 967, and 610 cm−1 are attributed to the v3, v1, v4 of SO42− vibration bands of ZnSO4Zn3(OH)6·nH2O65,66 and peaks at 876 and 450 cm−1 are related to the V–O and Zn–O bonds in ZnxV2O5 and Zn3(OH)2V2O7·2H2O.67 Therefore, the coexistence of ZnxV2O5 and byproducts, ZnSO4Zn3(OH)6·5H2O and Zn3(OH)2V2O7·2H2O, is concluded in the discharged V2O5 electrode. On the other hand, for the Zn counter electrode in a discharged cell, several peaks at 1129, 967, 566, 440, and 398 cm−1 are observed. The peaks appearing at 440 and 566 cm−1 are assigned to the Zn–O vibration of Zn1+xO on the surface of Zn metal,65,68 while 1129, 967, and 398 are assigned to the v3, v1, v4 of SO42− vibration in the ZnSO4Zn3(OH)6·nH2O.65,66 Upon charging, the spectrum of fully charged V2O5 at 1.6 V returns back to its main original features with less intensity, indicating the disappearance of ZnxV2O5 and the byproducts, ZnSO4Zn3(OH)6·5H2O and Zn3+δ(OH)2V2O7·2H2O. This demonstrates the reversible reaction during Zn-ion insertion and deinsertion as identified by in operando synchrotron diffraction and XAS. Moreover, an additional broad peak at 875 cm−1 related to ZnxV2O5 is observed for the counter electrode Zn from a charged cell, compared with that from a discharged one. This indicates that the byproduct ZnSO4Zn3(OH)6·5H2O does not completely disappear on the surface of Zn metal. Dissolved ZnxV2O5 can pass through the separator and reaches the surface of Zn metal. This contributes to ongoing degradation and limits the cycling stability.
![]() | ||
| Fig. 6 Raman spectra of pristine V2O5, the 1st discharged and charged state of V2O5 and of the Zn counter electrode from a discharged and charged cell. | ||
TEM and elemental mapping were carried out to further study the structural and morphology evolution of V2O5 during cycling. It is unable to observe the nanowire-like feature of ZnxV2O5 on the fully discharged electrode, whereas a sheet-like morphology can be clearly seen (Fig. 7a). Fig. S6† shows that the O, S, V, and Zn elements are uniformly distributed in the sheet-like material. The sheet-like material is probably attributed to the byproducts of ZnSO4Zn3(OH)6·5H2O, as demonstrated by synchrotron diffraction. Fig. 7b confirms the disappearance of sheet-like morphology and the recovery of nanowire-like feature of V2O5 after the charge process, demonstrating the decomposition of byproducts.
XPS was applied to investigate the surface chemistry and surface elemental composition of pristine V2O5, first discharged V2O5, and first recharged V2O5. As displayed in Fig. 8, the V 2p spectrum of pristine V2O5 can be fitted with two doublets: a main one with V 2p3/2 at 517.6 eV and a second one with weak intensity at 516.3 eV, which demonstrates that V exists mainly in the oxidation state +5 with a minor contribution of vanadium +4. It can be seen that the O 1s spectrum of pristine V2O5 can be fitted with one peak at 530.3 eV, corresponding to V–O group. The V 2p spectrum in the discharged state is not visible anymore due to the formation of the byproduct ZnSO4Zn3(OH)6·5H2O on the surface of the electrode, which blocks photoelectrons. While the V 2p spectrum of the charged state exhibits two V 2p3/2 components at 517.7 and 516.4 eV, the spectrum returns back to the one of pristine V2O5 after charge. For the discharged state of V2O5, a symmetric O 1s spectrum at 532.0 eV is obtained, assigning to the OH− and SO42− group of the byproduct ZnSO4Zn3(OH)6·5H2O, which was formed on the surface of the electrode and makes the O 1s spectrum from buried V–O groups invisible. After charging, the O 1s spectrum of the V–O group is visible again, accompanied by a minor contribution of OH− on the surface of the electrode.
![]() | ||
| Fig. 8 V 2p and O 1s X-ray photoelectron spectra of pristine V2O5, together with the 1st discharged and the 1st charged state. | ||
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ta03518e |