Binbin
Chang
a,
Yanzhen
Guo
c,
Donghai
Wu
c,
Li
Li
*a,
Baocheng
Yang
*c and
Jianfang
Wang
*b
aShanghai Key Laboratory of Green Chemistry and Chemical Processes, School of Chemistry and Molecular Engineering, East China Normal University, Shanghai 200241, China. E-mail: lli@chem.ecnu.edu.cn
bDepartment of Physics, The Chinese University of Hong Kong, Shatin, Hong Kong SAR, China. E-mail: jfwang@phy.cuhk.edu.hk
cHenan Provincial Key Laboratory of Nanocomposites and Applications, Institute of Nanostructured Functional Materials, Huanghe Science and Technology College, Zhengzhou 450006, China. E-mail: baochengyang@infm.hhstu.edu.cn
First published on 20th July 2021
Benefiting from the superior conductivity, rich surface chemistry and tunable bandgap, Ti3C2 MXene has become a frontier cocatalyst material for boosting the efficiency of semiconductor photocatalysts. It has been theoretically predicted to be an ideal material for N2 fixation. However, the realization of N2 photofixation with Ti3C2 as a host photocatalyst has so far remained experimentally challenging. Herein, we report on a sandwich-like plasmon- and an MXene-based photocatalyst made of Au nanospheres and layered Ti3C2, and demonstrate its efficient N2 photofixation in pure water under ambient conditions. The abundant low-valence Ti (Ti(4−x)+) sites in partially reduced Ti3C2 (r-Ti3C2) produced by surface engineering through H2 thermal reduction effectively capture and activate N2, while Au nanospheres offer plasmonic hot electrons to reduce the activated N2 into NH3. The Ti(4−x)+ active sites and plasmon-generated hot electrons work in tandem to endow r-Ti3C2/Au with remarkably enhanced N2 photofixation activity. Importantly, r-Ti3C2/Au exhibits ultrahigh selectivity without the occurrence of competing H2 evolution. This work opens up a promising route for the rational design of efficient MXene-based photocatalysts.
Nitrogen photofixation offers an approach for achieving the energy-saving and environmentally friendly NH3 synthesis under ambient conditions with renewable solar energy as the driving force.8–10 In N2 photofixation, H2 is replaced by H2O as a reducing agent. N2 and 3H2O are converted to 2NH3 and 1.5O2.11–17 The key is to design an efficient photocatalyst. Two-dimensional (2D) photocatalysts exhibit unique merits in solar-to-chemical energy conversion.18–22 MXenes, a family of 2D layered transition metal carbides, nitrides or carbonitrides, have aroused much interest since the first report in 2011.23 Benefiting from the metallic conductivity, abundant surface terminal groups, large surface-to-volume ratio, excellent hydrophilic and ion transport properties, MXenes have been explored in diverse fields.24–26 Ti3C2, the first reported MXene, possesses several unique characteristics.24,25 (i) Its high conductivity enables excellent charge transfer kinetics, favoring the rapid migration and efficient separation of photogenerated electrons and holes; (ii) abundant exposed metal sites offer many active sites for catalysis; (iii) adjustable terminal groups (OH, O, F, etc.) bring a tunable bandgap and optical absorption, enabling facile regulation of the photocatalytic performance; (iv) excellent surface hydrophilicity improves the interfacial connection with other materials, facilitating the formation of heterostructures. Ti3C2 has therefore become a research hotspot in photocatalysis.27–30 Theoretical calculations have shown that Ti3C2 presents valid N2-philicity and the ability to chemisorb and activate N2, suggesting that Ti3C2 can be a promising material for N2 capture and reduction.31 Unfortunately, the extremely low Fermi level and metallic nature of Ti3C2 make it a superior electron acceptor, resulting in a poor separation efficiency of photogenerated electrons and holes.32,33 In addition, the narrow bandgap of Ti3C2 makes N2 photoreduction difficult.34 As a result, it has remained challenging to realize N2 photofixation solely with Ti3C2.
Plasmonic metal nanoparticles possess extraordinary optical properties that arise from localized surface plasmon resonance (LSPR) and offer a powerful means for boosting the photocatalytic activity.18,35 LSPR-enhanced photocatalysis mainly relies on the extension of light absorption to the long-wavelength range and the enhancement of the local electric field. Plasmonic hot electrons can drive reduction reactions and improve photocatalytic NH3 synthesis.18,36–38 The plasmon-intensified electric field can promote the photogeneration of charge carriers in semiconductors.39,40 As a result, combining plasmonic metal nanoparticles with 2D MXenes is expected to be a feasible strategy for constructing efficient photocatalysts for NH3 production.
Herein, we report on the construction of a Au nanosphere-embedded, partially reduced, and layered Ti3C2 (r-Ti3C2) photocatalyst with a unique sandwich-like architecture for efficient N2 photofixation under ambient conditions. r-Ti3C2 shows an expanded layer spacing and exposes many low-valence Ti sites (Ti(4−x)+) on the edge and basal planes, which serve as active sites for N2 activation. The unique sandwich-like, Au nanosphere-embedded r-Ti3C2 not only provides a large number of Ti(4−x)+ active sites but also brings a high contact area between Au nanospheres and r-Ti3C2, improving the probability of excited charge carriers to interact with the reaction solution. Moreover, the embedding of Au nanospheres hinders the self-stacking of the r-Ti3C2 layers, benefiting the exposure of the active sites and boosting the effective utilization of the active sites and charge carriers. The hot electrons photoexcited on the plasmonic Au nanospheres inject into r-Ti3C2 and thereby reduce Ti(4−x)+ site-activated N2 into NH3. The charge carrier recombination is largely suppressed because the electrons and holes are located in r-Ti3C2 and the Au nanospheres, respectively. The photocatalysts exhibit a superior activity for N2 photofixation in pure water at ambient temperature and pressure. Our strategy opens up new opportunities for designing MXene/(plasmonic metal) nanostructures to achieve efficient photo-driven N2 fixation.
Scanning electron microscopy (SEM) imaging (Fig. 1b) reveals the accordion-like multilayered structure of Ti3C2, suggesting the successful etching of the Al layers. The layered texture is well kept in r-Ti3C2 (Fig. 1c), indicating that the H2 treatment does not deteriorate the original layered structure. The Au nanospheres dispersed in aqueous solutions exhibit an extinction peak at 518 nm (Fig. S3†). Their sizes are uniform (Fig. 1d), as revealed by transmission electron microscopy (TEM), with an average diameter of 12.8 ± 0.7 nm (Fig. S4†). In the low-magnification SEM images of Ti3C2/Au and r-Ti3C2/Au (Fig. S5†), a unique sandwich-like architecture is clearly observed. The Au nanospheres are interlaminated between the MXene layers and uniformly distributed on the basal planes. High-magnification SEM imaging further shows clearly that the Au nanospheres are uniformly interlaminated in the MXene layers (Fig. 1e and f). The X-ray diffraction (XRD) of Ti3AlC2 (Fig. S6a†) reveals a strong and typical diffraction pattern of the pure Ti3AlC2 phase (JCPDS no. 52-0875). After HF treatment, the strong (002) peak exhibits a downshift from 9.55° to 9.05°, which corresponds to a c-lattice parameter (c-LP) increase from 18.53 Å to 19.48 Å, implying an interlayer spacing of 0.98 nm in Ti3C2. In addition, the disappearance of the intense peak at 2θ = 39.08° in Ti3AlC2 after HF etching verifies the removal of the Al layers.42 Taken together, these results confirm the successful synthesis of Ti3C2 MXene. After H2 reduction, r-Ti3C2 displays a similar XRD pattern to Ti3C2 (Fig. 1g), except an additional (006) diffraction peak at 2θ = 28.5° (Fig. S6b†), reflecting a better-organized multilayered structure with more opened Ti3C2 layers.43 The XRD patterns also reveal the coexistence of the cubic Au phase (JCPDS no. 01-1172) and Ti3C2 in Ti3C2/Au and r-Ti3C2/Au (Fig. 1g). Compared to Ti3C2, the (002) peak shows clear and different shifts among r-Ti3C2, Ti3C2/Au and r-Ti3C2/Au (Fig. 1h). A slight shift of the (002) peak to a higher angle of 9.12° for r-Ti3C2 corresponds to a c-LP decrease from 19.48 Å to 19.25 Å, signifying a reduced interlayer spacing of 0.96 nm in r-Ti3C2. The small c-LP change of r-Ti3C2 can be ascribed to the elimination of H2O molecules interlaminated between the Ti3C2 layers or surface reactions during H2 reduction.23,44 The (002) peak shifts down to 2θ = 8.95° for sandwich-like Ti3C2/Au and r-Ti3C2/Au, which corresponds to a c-LP of 19.68 Å, indicative of an enlarged interlayer spacing of 1.00 nm. The increased interlayer spacing is probably caused by the intercalation of the Au nanospheres between the Ti3C2 and r-Ti3C2 segments.45 Each segment contains multiple Ti3C2 layers, but its overall thickness is greatly reduced in comparison with the sample before the intercalation of the Au nanospheres. In the Raman spectra of Ti3AlC2 (Fig. S7†), four major peaks appearing at 145, 260, 410 and 605 cm−1 are the characteristic Raman bands of Ti3AlC2. They arise from the ω1, ω2, ω3 and ω4 Raman-active vibrational modes.46,47 Ti3C2 and r-Ti3C2 show similar Raman peaks, with a highly intensified peak at 153 cm−1, along with three weak peaks at 260, 428 and 610 cm−1. All the four peaks can be ascribed to the Raman-active vibrational modes of Ti–C,48,49 suggesting the successful etching of the Al atoms and the preservation of the Ti3C2 layers. In addition, two broad bands observed at 1350 and 1610 cm−1 for Ti3C2 and r-Ti3C2 correspond to the D- and G-bands of carbon, manifesting the existence of disordered carbon and ordered graphitic carbon, respectively. The larger peak intensities of the D- and G-bands in r-Ti3C2 reveal the existence of more disordered carbon after H2 reduction, suggesting the formation of more oxygen defects in the carbon layers of r-Ti3C2.50 Such oxygen defects can bring more active sites for N2 adsorption on the surface of r-Ti3C2.
Ti3C2 shows clear absorption in the spectral region of 300–800 nm with a maximum at ∼520 nm (Fig. 1i). r-Ti3C2 also exhibits a broad absorption band in the region of 300–800 nm, but the absorption maximum exhibits a slight redshift. This phenomenon is probably caused by the changes in the surface chemistry and terminal groups of r-Ti3C2, resulting in a changed bandgap.51 Despite the broad light absorption, very few charge carriers can be photogenerated and separated in Ti3C2 and r-Ti3C2.32–34 On the other hand, the efficient photothermal conversion of Ti3C2 MXene can facilitate surface catalytic reactions through the conversion of light to heat to activate the supported catalyst.52 Unlike common plasmonic Au/semiconductor hybrid photocatalysts,36,53 the absorption peak from the LSPR band of the Au nanospheres cannot be clearly observed in Ti3C2/Au or r-Ti3C2/Au. This result is likely caused by the spectral overlap between the LSPR of the Au nanospheres and the strong broad absorption of Ti3C2 MXene, which is reflected by the enhanced absorption in the region of 500–600 nm. The charge transport ability is another key factor in photocatalysis. Electrochemical impedance spectroscopy (EIS) measurements were conducted under white light illumination in a N2 atmosphere (Fig. S8†). A smaller semicircle in the obtained Nyquist plot implies a better charge transfer capability at the electrode–electrolyte interface. r-Ti3C2/Au exhibits the smallest arc radius, signifying a good charge transfer ability. The improved charge transfer ability can be attributed to the effective interfacial charge transfer in the sandwich-like r-Ti3C2/Au. Though the metallic Ti3C2 is difficult to photogenerate charge carriers, it can serve as an electron acceptor to capture the hot electrons generated by the plasmonic Au nanospheres owing to its superior electrical conductivity.32
To verify the nitrogen and proton sources of the produced NH3, control experiments were carried out with r-Ti3C2/Au (Fig. S11†). NH4+ was not detected when N2 or H2O was replaced with Ar or aprotic acetonitrile, suggesting that the nitrogen and proton sources for the NH4+ formation are from N2 and H2O, respectively. In addition, NH4+ cannot be generated in dark, suggesting that light is an essential driving force for N2 photofixation. To further corroborate the origin of the produced NH3, an isotope labeling experiment was performed using 14N2 and 15N2 as the nitrogen sources. The obtained 14NH4Cl and 15NH4Cl were measured by 1H nuclear magnetic resonance (NMR) spectroscopy (Fig. 3a). The triplet and doublet peaks corresponding to 14NH4+ and 15NH4+ can be clearly observed in the 1H NMR spectra of the photocatalytic reaction solutions when 14N2 and 15N2 were used as the feed gas, respectively. This result verifies that the produced NH4+ indeed originated from N2 photofixation. Moreover, the evolution of O2 was also detected during the N2 photofixation process in a sealed reactor (Fig. S12a†). To assess whether O2 was produced during the N2 photofixation reaction catalyzed by r-Ti3C2/Au, the reactor was evacuated, bubbled with N2, and then sealed. Upon illumination for 1 h under white light, O2 was detected. The generated O2 should result from the oxidization of H2O by the hot holes in the Au nanospheres.54 Its amount is about three fourths that of NH4+ (Fig. S12b†), close to the stoichiometric ratio of 3:4 according to the reaction N2 + 3H2O → 2NH3 + 1.5O2, proving that NH3 is generated by coupling the activated N2 with the protons from H2O. Importantly, H2 was not detected during the N2 photofixation process (Fig. S12a†), suggesting the absence of the competing hydrogen evolution reaction. r-Ti3C2/Au is therefore a highly selective photocatalyst for N2 fixation.
To reveal the mechanism of the photocatalytic N2 fixation, photocurrent tests were first performed under white light illumination in both N2 and Ar atmospheres (Fig. 3b). For Ti3C2, the photocurrent densities measured in Ar and N2 are nearly the same and reach ∼0.76 µA cm−2 (Fig. 3c). The photocurrent density of r-Ti3C2 is similar to that of Ti3C2, and the photocurrent in N2 shows a slight reduction. In the presence of the Au nanospheres, the photocurrents of Ti3C2/Au and r-Ti3C2/Au are enhanced in Ar because of the LSPR effect, and both reach ∼1.65 µA cm−2. There is a small decrease of ∼0.15 µA cm−2 in the photocurrent density of Ti3C2/Au when the Ar atmosphere changed to N2, which means a slight electron consumption for the reduction of N2 molecules. Remarkably, the photocurrent density of r-Ti3C2/Au in N2 is only one fifth of that in Ar, suggesting that the four fifth difference in photocurrent is consumed to reduce N2 molecules. As a result, r-Ti3C2/Au displays a remarkable N2 photofixation activity (Fig. 2). To look into the reaction process of adsorbed H2O and N2 and prove the activation and reduction of N2 on the surface of r-Ti3C2/Au, in situ diffuse-reflectance infrared Fourier transform spectroscopy (DRIFTS) was employed to monitor the N2 photofixation process. To record the DRIFT spectra, r-Ti3C2/Au was exposed to water vapor-saturated N2 under white light illumination, which allows for the investigation of the time-dependent change of the molecular species adsorbed on the catalyst. In the control experiment performed in an Ar atmosphere, two clear absorption peaks at 1660 and 3580 cm−1, corresponding to the characteristic bending modes of adsorbed H2O molecules,36 were observed. Their intensities were enhanced as the reaction time was prolonged (Fig. 3d). No absorption bands related to the N-containing species were detected, which further indicates that the nitrogen in NH3 truly originated from N2 molecules. The time-dependent DRIFT spectra recorded after the injection of N2 under white light reveal that several absorption peaks gradually appear as the illumination time was prolonged from 0 to 6 h. The signal at 2340 cm−1 can be ascribed to strongly chemisorbed N2 molecules.55 The absorption band at 2032 cm−1 is believed to arise from the Ti–NN complex formed through N2 binding to the Ti3+ sites.56 The absorption band at ∼3160 cm−1 corresponds to the adsorbed ammonia.9,37 Furthermore, the characteristic absorption band at 1410 cm−1 assigned to the NH4+ deformation vibration is intensified with increasing illumination time.37,57 These DRIFTS results provide strong evidence that N2 molecules can be adsorbed, activated and further reduced to form NH4+ under light illumination.
To further understand the photocatalytic N2 fixation performance of r-Ti3C2/Au, the effect of the Au nanosphere amount in r-Ti3C2/Au was systematically investigated. The amount of embedded Au nanospheres was determined by inductively coupled plasma mass spectrometry (ICP-MS; Fig. S13†). Fig. 4a shows the high-magnification SEM images of the Au/r-Ti3C2 samples that were embedded with the 12.8 nm-sized Au nanospheres at 0.49, 1.11, 1.78 and 2.28 wt% relative to the total amount of Au and r-Ti3C2, respectively. The unique sandwich-like architecture is observable for all samples. The Au nanospheres are uniformly distributed on the basal planes even when the loaded Au amount is increased to 1.78 wt%. As the embedded Au amount is increased to 2.28 wt%, aggregation occurs. The NH4+ concentrations catalyzed by the Au/r-Ti3C2 samples with different Au amounts increase with the illumination time under white light (Fig. 4b). When the embedded Au amount is increased from 0.49 to 1.78 wt%, the produced NH4+ amount steadily increases within the same reaction time. The r-Ti3C2/Au sample with the Au amount of 1.78 wt% gives the highest amount of the produced NH4+, whose concentration reaches 307.8 µmol L−1 in 6 h. However, when the embedded Au amount is further increased to 2.28 wt%, the generated NH4+ concentration is clearly reduced. Similarly, the normalized NH4+ production rate first increases with the Au amount, reaches the highest value of 31.8 µmol h−1 gcat−1 at the loaded Au amount of 1.78 wt%, and then decreases (Fig. 4c). To further explore the relationship between the N2 photofixation activity and the LSPR effect of the Au nanospheres, r-Ti3C2/Au with different Au nanosphere sizes and amounts were prepared. The uniform Au nanospheres with average sizes of 16.1 ± 0.8 (Fig. S14†) and 21.0 ± 0.8 nm (Fig. S15†) were synthesized. The unique sandwich-like structure with the uniform distribution of the Au nanospheres in the interlayers was obtained. Similarly, a high Au amount results in a reduction in the NH4+ production. Fig. 4d summarizes the relationship between the NH4+ generation rate and the loaded Au nanosphere size and amount. For the same Au size, the NH4+ production rates show a nearly volcano-shaped dependence on the embedded Au amount. An optimal N2 photofixation performance is achieved at a particular Au amount, which increases with the Au nanosphere diameter. The optimal Au amount for each size can be attributed to the enhanced LSPR effect with increasing amounts of Au nanospheres. The decrease in the N2 photofixation rate at a higher Au amount should be caused by the aggregation of the Au nanospheres and/or the blocking of the active sites on r-Ti3C2 for N2 adsorption by the excessive Au nanospheres. The N2 photofixation rates for the r-Ti3C2/Au samples containing the 20 nm-sized Au nanospheres are generally smaller than those of the samples containing the 13 nm- and 16 nm-sized Au nanospheres. This is probably because the number of Au nanospheres plays a more important role than the absorption cross-section for the LSPR effect in N2 photofixation. The optimal sample was found to be r-Ti3C2/Au containing the 16 nm-sized Au nanospheres at 2.45 wt%. This sample gives a NH4+ production rate of 33.8 µmol h−1 gcat−1.
Au nanospheres capped with different molecules were next employed to study their assembly with r-Ti3C2 and in turn their effect on N2 photofixation. Au nanospheres coated with cetyltrimethylammonium bromide (CTAB) were chosen. They exhibit good dispersibility and uniform sizes with an average diameter of 19.8 ± 0.7 nm (Fig. S16†). The CTAB-capped Au nanospheres were found to predominantly assemble onto the edges of the r-Ti3C2 layers (Fig. 5a). The resultant sample is therefore denoted r-Ti3C2/edge-Au. The CTAB-capped Au nanospheres are positively charged with a zeta potential of +34.2 mV, and the layered r-Ti3C2 sample is negatively charged with a zeta potential of −28.8 mV (Fig. S17†). The two components can therefore spontaneously assemble together through electrostatic attraction during solvent evaporation. The assembly results in an intimate contact between the Au nanospheres and the edges of r-Ti3C2. It also implies that the electrostatic attraction force is stronger than the solvent-driven force. In contrast, the citrate-capped Au nanospheres cannot be adsorbed onto the edges of r-Ti3C2 due to electrostatic repulsion. They are driven into the interlayers of r-Ti3C2 by the solvent, producing the sandwich-like nanostructure. The SEM images (Fig. 5b) of r-Ti3C2/edge-Au reveal that the Au nanospheres are distributed along the edges of the layered r-Ti3C2 without clear aggregation, even when the Au amount is increased from 1.25 to 3.75 wt%. The N2 photofixation activity of r-Ti3C2/edge-Au increases with increasing Au amounts (Fig. S18†). The photocatalytic N2 fixation performances of r-Ti3C2/Au with the Au nanospheres located at different positions are compared under the identical nanosphere diameter of ∼20 nm and the close amounts of Au (Fig. 5c). Considerable reductions in the NH4+ production rate are seen for the r-Ti3C2/edge-Au catalysts. The reductions are probably caused by the relatively large average distance from the edge-positioned Au nanospheres, which act as the electron sources, to the active sites on the layers of r-Ti3C2. The large distance increases the probability for electrons to get lost during their transport.
Density functional theory (DFT) calculations were performed to investigate the chemisorption and activation of N2 molecules on different Ti sites of Ti3C2 MXene (Fig. 6f). Upon adsorption of a N2 molecule on the Ti1 site, the optimized N2 coordination configuration shows that the N2 molecule is chemisorbed on a Ti–Ti tripolymer center through a dinuclear end-on coordination mode, in which one N atom binds with the Ti–Ti tripolymer and the other binds with the Ti–Ti dimer (Fig. 6g). When a N2 molecule is adsorbed on the Ti2 site, the optimized coordination configuration is similar to that of N2 coordinated to the Ti1 site, but the adjacent two Ti1 sites are combined to form a Ti1–Ti2 tripolymer and a Ti1–Ti2 dimer (Fig. 6g). The Ti3 and Ti4 sites cannot adsorb N2 molecules (Fig. 6g), which is probably caused by the weak interaction due to the strongly electronegative nature of the surface O-terminal groups.61 To disclose the electron transfer between r-Ti3C2 and the adsorbed N2, the charge density difference was calculated (Fig. 6g, bottom row). A clear charge density difference is observed for the Ti1 and Ti2 sites, suggesting the occurrence of electron transfer from r-Ti3C2 to the N2 molecule. The electron-enriched isosurface on the adsorbed N2 molecule exhibits a π-orbital feature, indicating that the d-orbital electrons on the adjacent Ti atoms at the Ti1-site are transferred to the captured N2 molecule. As electrons are injected into the N2 molecule, the NN triple bond is considerably weakened with an elongated bond length. The triple bond lengths of the N2 molecules adsorbed at the Ti1 and Ti2 sites, respectively, increased to 1.351 and 1.345 Å, much longer than the value of 1.114 Å for a free N2 molecule (Fig. S20a and b†). In addition, a distinct reduction in the electron density between the two N atoms is also observed, implying that electrons are donated from the highest occupied σ-orbital of the N2 molecule to the adjacent Ti sites. Such phenomena of electron donation from N2 to the metal and back-donation from the metal to N2 also happen in M (transition metal)–N2 complexes and have been discovered for many metals.1,62,63 The strong activation of N2 molecules through electron back-donation from transition metals with available d-orbital electrons plays a crucial role in boosting the photocatalytic N2 fixation activity of the r-Ti3C2 catalyst.
In order to better understand the N2 chemisorption, we also performed DFT calculations to examine the adsorption energy (Ead) of N2 at different sites on r-Ti3C2 MXene (Fig. S20†). A comparison of the Ead values of a N2 molecule at the Ti1 site with different adsorption configurations reveals that the optimal N2 coordination configuration mentioned above gives the largest Ead value of −3.525 eV, meaning that N2 activation can be spontaneously realized when it is adsorbed at the Ti1 site. A comparison of the Ead values of N2 at different sites (Fig. S20†) shows that Ti1 is the strongest active site for N2 adsorption in r-Ti3C2 MXene. In addition, the adjacent Ti1 sites can help to build the optimal coordination configuration for N2 activation. The more the Ti1 sites are involved, the higher the Ead value is. Moreover, the Ti1 site does not bond with any O atoms. The bond length and adsorption energy of the N2 molecule at the Ti1 site obtained in our calculations for Ti3C2 MXene are very close to those obtained in previous works for Ti2C MXene.64,65
Based on the above results, we propose a reaction mechanism for photocatalytic N2 fixation with r-Ti3C2/Au under ambient conditions (Fig. 7e). Benefiting from the good hydrophilicity, the r-Ti3C2/Au photocatalyst can be stably and uniformly dispersed in water. r-Ti3C2 possesses numerous low-valence Ti(4−x)+ sites that are associated with OVs and generated through H2 thermal reduction. They are active sites for capturing and activating N2 molecules. Under light illumination, photogenerated hot electrons from the Au nanospheres are injected into r-Ti3C2, which subsequently reduce the activated N2 at the Ti(4−x)+ sites. The hot holes remaining on the Au nanospheres are consumed through the oxidation of H2O to produce O2. The produced NH3 is accumulated in the aqueous reaction solution.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1sc02772g |
This journal is © The Royal Society of Chemistry 2021 |