Photo-switching emission of photochromic materials has paramount importance in the field of optoelectronics. Here, we report synthesis and characterization of a dithienylethene (DTE) based photochromic low molecular weight gelator (LMWG) and self-assembly with lanthanide (Eu3+ and Tb3+) ions to form a photochromic coordination polymer gel (pcCPG). Based on DTE ring opening and closing, the TPY-DTE gel shuttles from pale-yellow coloured TPY-DTE-O to dark blue coloured TPY-DTE-C and vice versa upon irradiating with UV and visible light, respectively, and both the photoisomers show distinct optical properties. Furthermore, integration of Eu3+ and Tb3+ lanthanides with TPY-DTE resulted in red and green emissive Eu-pcCPG (Q.Y. = 18.7% for the open state) and Tb-pcCPG (Q.Y. = 23.4% for the open state), respectively. The photoisomers of Eu-pcCPG exhibit photo-switchable spherical to fibrous reversible morphology transformation. Importantly, an excellent spectral overlap of the Eu3+ centred emission and absorption of DTE in the closed form offered photo-switchable emission properties in Eu-pcCPG based on pcFRET (energy transfer efficiency >94%). Further, owing to the high processability and photo-switchable emission, the Eu-pcCPG has been utilized as invisible security ink for protecting confidential information. Interestingly, mixed Eu3+/Tb3+ pcCPG exhibited photo-modulated multi-spectrum chromism reversibly where the colour changes from yellow, blue, and red to green and vice versa under suitable light irradiation.
Here, we report the design and synthesis of a photochromic LMWG based linker (TPY-DTE) by integrating the DTE unit and terpyridine moiety through an amide linkage. TPY-DTE LMWG showed excellent photochromism in the gel state. Furthermore, two photochromic CPGs, Eu-pcCPG and Tb-pcCPG, were prepared by the self-assembly of Eu3+ and Tb3+ salts with TPY-DTE LMWG, respectively. A reversible morphological transformation between the microspheres and fibers was also demonstrated in the Eu-pcCPG along with the photochromic behaviour. Interestingly, Eu-pcCPG displayed fast photo-switchable emission properties based on a highly efficient pcFRET process (energy transfer efficiency = 94.79%). Further, highly processable photo-switchable emission Eu-pcCPG has been used as invisible security ink on ordinary paper and also exploited for decoding of confidential information. On the other hand, Tb-pcCPG did not exhibit photo-switchable emission; however, an optimized pcCPG of mixed metal Eu3+
:
Tb3+ (7
:
3 ratio) has shown interesting photo-modulated reversible emission as well as visible colour changes that can be employed for signalling and sensing applications.
:
6′,2′′-terpyridin]-4′-ylamino)propyl)-5-methylthiophene-2-carboxamide) (TPY-DTE), was synthesized by amide coupling between the DTE(COOH)2 photochrome and 2,2′
:
6′,2′′-terpyridin-4′-yl-propane-1,3-diamine (TPY-NH2) and characterized using different spectroscopic techniques (Fig. S1–S3†). UV-Vis absorption study for a methanolic solution (10−5 M) of yellow coloured TPY-DTE showed an overlap band in the range of 264–286 nm, which is attributed to π-π* transition for TPY30 and DTE(COOH)2 units60(Fig. S4†). Upon irradiation with UV light (λ = 365 nm) for 15 seconds, the yellow colour solution changes to blue because of the ring-closing of the DTE unit.54 The presence of additional absorbance between 500–700 nm in the UV-Vis absorption spectrum after UV irradiation further confirms the photocyclization of the DTE units in the LMWG (Fig. S4a†).5 Notably, saturation of DTE-ring closing was observed upon UV irradiation for ∼60 s (Fig. S4a†). Further, the photocycloreversion (DTE ring-opening) in TPY-DTE LMWG was observed upon visible light irradiation (λ > 400 nm), and completion of the reaction was achieved in ∼110 s (Fig. S4b†). The quantum efficiency for the conversion of the open to the closed form (TPY-DTE) and vice versa was calculated to be 81% and 69%, respectively (Fig. S4c and d†).37,38 Moreover, the maximum conversion of the open to the closed form in the photostationary state (PSS) upon UV-light irradiation was found to be ∼72%. The gelation propensity of LMWG was examined in various solvent systems under different conditions (Table S1, see the ESI† for details). For organogel (OG) preparation, the LMWG (5 mg) was taken in a 0.3 mL solvent mixture of methanol (0.2 mL), ethylene glycol (0.05 mL) and water (0.05 mL). The reaction mixture was heated gradually from 60 °C to 120 °C in a closed vial and subsequently cooled to room temperature which resulted in a pale yellow coloured organogel (OG) of TPY-DTE (Fig. 1a and S5–S7†). The gel can be converted to the sol form by heating at 80 °C, confirming the thixotropic behaviour (Fig. S7†). The yellow gel (TPY-DTE-GO i.e. gel in the open form) can be converted to the dark blue coloured gel (TPY-DTE-GC i.e. gel in the closed form) upon irradiating with UV-light for 10–15 seconds and can be reverted to yellow colour by treating with visible light for 25–30 seconds (Fig. 1a). The UV-Vis absorption spectra of TPY-DTE-GO also showed the overlap bands in the range of 264 nm to 290 nm, which are characteristic of the π–π* transition for both, TPY and DTE units (Fig. 1d). On the other hand, TPY-DTE-GC showed additional broad absorbance in the visible region with a maximum at 610 nm due to the ring closing of the DTE unit. The reversibility of photochromic behaviour of the TPY-DTE gel has been examined for ten cycles and found to be equally effective as for the 1st cycle, suggesting excellent fatigue resistance behaviour of the gel (Fig. 1d and S8a†). Similar to the TPY-DTE LMWG, upon continuous UV-light irradiation on the TPY-DTE-GO, UV-Vis absorption spectra were recorded in a time interval of three seconds, and the maximum conversion from TPY-DTE-GO to TPY-DTE-GC can be achieved in ∼60 seconds (Fig. S8b†).
Similarly, the complete reversible conversion of TPY-DTE-GC to TPY-DTE-GO can be achieved in ∼120 seconds with continuous visible light irradiation as confirmed by the UV-Vis absorption spectrum (Fig. S8c†). The reversible fast-photochromism in the TPY-DTE organogel as compared to previously reported DTE-based solid photochromic materials49,61 could be attributed to its gelacious nature, which provides more space for facile structural changes during the photo reaction.54 The powder X-ray diffraction (PXRD) pattern of the TPY-DTE-GO showed a peak at 2θ = 26.43°, corresponding to a d-spacing value of 3.36 Å which indicates the presence of π–π stacking in the self-assembly (Fig. S6†). Comparison of the FTIR spectra of TPY-DTE LWMG and the TPY-DTE-OG revealed a decrease in –C
O and –N–H stretching frequencies from 1696 cm−1 to 1684 cm−1 and from 3462 cm−1 to 3436 cm−1, respectively, indicating the presence of intermolecular H-bonding between the amide groups of DTE-TPY (Fig. S5†).62 The surface morphology of TPY-DTE-GO and TPY-DTE-GC was analyzed by FE-SEM (Fig. S9†). This showed irregular interconnected sheet-like morphologies for both cases, ensuring that the supramolecular architecture remains unaffected by the light treatment. This was further supported by the high-resolution TEM (HR-TEM) analysis as similar layered sheet type morphology was observed for both the photo-isomers (Fig. 1e and f). The rheology measurements for TPY-DTE-GO and TPY-DTE-GC showed that the storage modulus G′ was considerably higher than the loss modulus G′′ for both, indicating the elastic properties of the self-assembly, which is characteristic of a stable gel phase54 (Fig. 1c). Notably, an increase in the G′ value was observed for TPY-DTE-GC as compared to TPY-DTE-GO, which could be attributed to the greater mechanical strength due to stronger π–π stacking in the planar configuration of the closed-ring photoisomer.63 The photoconversion of TPY-DTE-GO to TPY-DTE-GC was further confirmed through IR spectra which showed a characteristic shift of CH3 bending linked to thiophene rings from 985 cm−1 to 996 cm−1 for open to closed form conversion (Fig. S5†).64,65 The quantum efficiency for the conversion of TPY-DTE-GO to TPY-DTE-GC and vice versa was calculated to be 60% and 46%, respectively (Fig. S10†).37 Moreover, the maximum conversion of TPY-DTE-GO to TPY-DTE-GC in the photostationary state (PSS) upon UV-light irradiation was found to be ∼71%. Owing to the excellent processability, we have exploited yellow coloured TPY-DTE-GO for writing applications by coating over an ordinary paper (Fig. 1g). The light-yellow gel-coated paper turned blue in colour upon UV-irradiation for ∼15 seconds and reverted to a light-yellow colour upon shining visible light for ∼30 seconds. Further, various designs have been made just in a few seconds upon UV-light irradiation through UV-masking, indicating the potential of the material to be used in the lithographic technique, ordinary UV-sensors, and writing applications37,55 (Fig. 1h).
:
1 (Fig. 2a) and showed the bathochromic shift of TPY absorption from 276 nm to 300 nm due to metal binding.66 The binding constant (Ka) for Eu3+ to TPY-DTE LMWG was calculated using the Benesi–Hildebrand plot67 and found to be 4.54 × 104 M−1 (Fig. S11†). Next, gelation was attempted with an equimolar ratio of Eu3+ and TPY-DTE under similar conditions as employed for TPY-DTE OG and resulted in the yellow coloured Eu-pcCPG-O (gel in the open form) (Fig. 2b and S12–S14†). FE-SEM and TEM analysis of Eu-pcCPG-O showed a nano-sized (300–600 nm) interconnected spherical morphology (Fig. 2d and e). EDAX analysis indicated the presence of 11.84 wt% Eu3+ in Eu-pcCPG-O, which is in good agreement with the theoretical prediction (Fig. S14a†). Elemental mapping demonstrated the uniform distribution of Eu3+ in the supramolecular network (Fig. S14b†). The PXRD pattern of Eu-pcCPG-O showed a low angle peak at 7.68° (d = 11.5 Å), indicating the formation of a higher-order self-assembled structure upon Eu3+ coordination to the TPY centre (Fig. S13†). Notably, PXRD peaks at 2θ = 24.53° (d = 3.6 Å) and 26.25° (d = 3.4 Å) indicated the presence of π–π stacking in the self-assembly in Eu-pcCPG-O (Fig. S13†). Further, FT-IR analysis revealed a significant shift in the C
O stretching frequency of Eu-pcCPG-O (ν = 1642 cm−1) in comparison to the TPY-DTE-GO (ν = 1684 cm−1) that can be attributed to the stronger H-bonding (i.e. C
O⋯H–N– interactions) in Eu-pcCPG-O which is also supported by the appearance of an intense peak at 3455 cm−1 for ν(N–H) (Fig. S12†). The UV-Vis absorption spectrum of the yellow Eu-pcCPG-O showed a subtle bathochromic shift as compared to that of TPY-DTE-GO and the absorption maximum was found to be at 310 nm. Next, irradiation of yellow coloured Eu-TPY-DTE-O pcCPG with UV-light for 30 seconds resulted in deep blue colouration due to the DTE ring-closing and confirmed the formation of the photo isomer Eu-pcCPG-C (gel in the closed form) (Fig. 2b). Eu-pcCPG-C revealed broad absorption in the visible range (500–750 nm) similar to TPY-DTE-GC (Fig. 2b). Importantly, visible light irradiation for 60 seconds caused blue Eu-pcCPG-C to further revert to yellow Eu-pcCPG-O. The UV-Vis absorption properties were examined back and forth from yellow (Eu-pcCPG-O) to blue (Eu-pcCPG-C) and vice versa upon irradiation with UV and visible light, respectively, for ten cycles and were found to be equally efficient as observed for the first cycle (Fig. S15†). The quantum efficiencies for the conversion of Eu-pcCPG-O to Eu-pcCPG-C and vice versa in the gel state were found to be 70% and 57%, respectively (Fig. S16†). The conversion ratio of Eu-pcCPG-O to Eu-pcCPG-C in the photostationary state (PSS) was calculated to be ∼71%. Next, the morphology of Eu-pcCPG was studied by TEM analysis with UV and visible light irradiation (Fig. 2e and f). Interestingly, upon UV light irradiation on the Eu-pcCPG-O for 2 min, the aggregated nanospheres were transformed into interconnected nanofibrous structures due to DTE ring-closing (Fig. 2f). Further, the reversibility of the morphology was investigated by visible light irradiation on the Eu-pcCPG-C. The regaining of the nano spherical morphology was achieved upon visible light irradiation for 10 min (Fig. 2g). This exclusive photoinduced reversible morphology transformation from spheres to fibers could enable the use of such materials in the domains of photoactuators4,39 and delivery media.45,68 Next, a rheology study was performed for Eu-pcCPG-O and Eu-pcCPG-C, which showed the viscoelastic nature of both the photoisomers of pcCPG. Notably, G′ for both Eu-pcCPG-O and Eu-pcCPG-C was found to be similar under less % strain, which decreases along with an increase in the % strain. The decrease is more pronounced from 0.02% to 0.1% strain for Eu-pcCPG-C which suggested the lower mechanical strength of the Eu-pcCPG-C as compared to Eu-pcCPG-O (Fig. 2c). Next, upon excitation at 310 nm, the Eu-pcCPG-O exhibited Eu3+ centred red emission at 590 (5D0–7F1), 615 (5D0–7F2), 652 (5D0–7F3), and 700 (5D0–7F4) nm54 (Fig. 3a). This can be easily discerned by the naked eye. Interestingly, the highest intensity emission peak of Eu3+ at 615 nm has excellent overlap with the absorption of Eu-pcCPG-C; thus, reversible photo-switchable luminescence of Eu-pcCPG can be realized based on a pcFRET process (Fig. 3a). The emission of Eu-pcCPG-O was almost quenched upon continuous UV irradiation for 70 s (Fig. 3b–e), which can be attributed to the formation of Eu-pcCPG-C. Furthermore, visible light irradiation on the blue-coloured Eu-pcCPG-C for 300 seconds revealed the reversion to yellow coloured Eu-pcCPG-O along with complete recovery of the corresponding Eu3+ based red emission (Fig. 3c and f). The DTE-ring opening was further confirmed by the absence of the absorption band in the range of 500–750 nm in the UV-Vis absorption spectrum of the obtained yellow Eu-pcCPG-O (Fig. 2b). The absolute quantum yields for Eu-pcCPG-O and its photo-isomer, Eu-pcCPG-C, were found to be 18.7% and 0.52%, respectively. Next, the rate constant has also been calculated for quenching and regaining of fluorescence by irradiating Eu-pcCPG (Fig. 3e and f). The change in the emission intensity was monitored at 615 nm, and the rate constant for fluorescence quenching and regaining was calculated to be 5.89 × 10−2 s−1 and 9.09 × 10−3 s−1, respectively (Fig. 3e and f). The rate constant study showed that DTE ring-opening takes a longer time as compared to ring-closing in Eu-pcCPG. Further, excited-state lifetimes were measured for Eu-pcCPG-O and its photo-irradiated form, Eu-pcCPG-C, upon excitation at 310 nm (Fig. 3g). The data of the lifetime for Eu-pcCPG-O and Eu-pcCPG-C were fitted using bi-exponential decay,69 indicating the presence of two distinct emitting centres which are most likely to appear due to two different coordination environments around the Eu3+ centre in the Eu-pcCPG. The Eu3+ centre in Eu-pcCPG carries two terpyridine units (occupying six coordination sites) and the remaining two coordination sites could be occupied by the water or nitrate anions or both (one water and one nitrate anion),70,71 which leads to the Eu3+ centres in two different coordination environments. This would change the ligand field strength around the Eu3+ centre in Eu-pcCPG that eventually results in the biexponential decay. The average lifetimes for Eu-pcCPG-O and Eu-pcCPG-C were calculated to be 397.0 μs and 20.7 μs, respectively (see the ESI for details and Table S2†). The significantly decreased excited-state lifetime of Eu-pcCPG-C provided strong support for the pcFRET process. The energy transfer efficiency calculated from the excited-state lifetime was found to be 94.79% (see the details in the ESI†). This further validated the existence of strong pcFRET in the Eu-pcCPG.
:
1 for Tb3+ with LMWG (Fig. S18a†). Similar to Eu-pcCPG, the binding constant (Ka) for Tb3+ to TPY-DTE LMWG was determined and found to be 5.05 × 104 M−1 (Fig. S18b†). The Tb3+ coordinated pcCPG gel (Tb-pcCPG) was prepared and characterized by adopting similar procedures and techniques as employed for Eu-pcCPG (see the details in the ESI†). Tb-pcCPG also showed photochromic behaviour based on DTE ring-opening/closing (Fig. S21†). Yellow coloured Tb-pcCPG-O can be converted to blue Tb-pcCPG-C by UV-irradiation which can be reverted by visible light treatment. The PXRD pattern and FT-IR spectrum of Tb-pcCPG-O was found to be similar to those of the Eu-pcCPG-O (Fig. S19 and S20†). This indicates the presence of π–π interaction and H-bonding in the self-assembly of Tb-pcCPG-O, similar to the Eu-pcCPG-O. FESEM and TEM analyses of Tb-pcCPG-O showed the interconnected spherical morphology similar to the Eu-pcCPG-O (Fig. S22†). The elemental mapping of Tb-pcCPG-O showed uniform distribution of Tb3+ (Fig. S23†), whereas EDAX analysis revealed the presence of 11.08 wt% Tb in Tb-pcCPG-O (Fig. S23†). Notably, upon excitation at 310 nm, Tb-pcCPG-O displayed four Tb3+ centred emission peaks with maxima at 490 (5D4–7F3), 546 (5D4–7F4), 587 (5D4–7F5), and 623 (5D4–7F6) nm (Fig. 5a). The highest intensity peak among all four bands was observed at 546 nm corresponding to 5D4–7F4 transition and responsible for the green emission of Tb-pcCPG-O.56 Importantly, emission of Tb-pcCPG-O has a poor overlap with the absorption of the closed form of Tb-pcCPG-C, and therefore, an effective pcFRET was not observed (Fig. 5a). This was further evident as UV irradiation for 60 seconds on the Tb-pcCPG-O showed insignificant emission quenching in Tb-pcCPG-C and the bright green emission remained intact (Fig. 5b and S21a†). Moreover, the quantum yield of Tb-pcCPG before and after UV irradiation remained similar and was found to be 23.4% and 21.1%, respectively. The decay profile for the excited-state lifetime for the photoisomers of Tb-pcCPG was found to be biexponential, similar to that of the Eu-pcCPG. The lifetime value for Tb-pcCPG-O and Tb-pcCPG-C was calculated to be 87.0 μs and 82.7 μs, respectively, indicating inefficient pcFRET (energy transfer efficiency = 4.94%) in this case (Fig. 5c, Table S3†).
Furthermore, as mentioned above, the emission of Tb-pcCPG was not photo-switchable and remained intact in the presence and absence of UV-light. Therefore, we were interested in examining the emission outcome of a gel based on a mixed metal (Eu/Tb-pcCPG) system. The optimized gel of Eu
:
Tb (7
:
3 ratio) pcCPG-O was obtained upon heating at 80 °C (see the details in the ESI†). The Eu/Tb-pcCPG-O excited at 310 nm showed distinct peaks for both Eu3+ and Tb3+ (Fig. S24†). However, bright red emission for Eu/Tb-pcCPG-O was detected by the naked eye due to the higher concentration of Eu3+ ions (Fig. 5d). Interestingly, owing to the photo-switchable emission properties of Eu-pcCPG, UV-irradiation on the mixed gel (Eu/Tb-pcCPG) system for 40 seconds resulted in quenching of red emission and yielded bright green emission that can be assigned to Tb-pcCPG-C. Notably, this green emissive mixed-gel was blue in colour under daylight. The emission spectrum recorded after UV-irradiation on the mixed gel sample showed Tb3+-centred emission. Thus, emission of a mixed lanthanide-based gel has been modulated reversibly upon light treatment, which is yet to be explored for the CPG system. Therefore, photo-modulated reversible colour changes, yellow ↔ red ↔ green ↔ blue ↔ yellow, can be achieved for Eu/Tb-pcCPG upon shining suitable light which is unprecedented in CPG systems (Fig. 5d). These photo-modulated emission and visible colour changes of mixed Eu/Tb-pcCPG can be employed for signalling applications.50,54
:
3 ratio) showed excellent reversible photo-modulated luminescence as well as photochromism that can be utilized for signalling applications. Owing to the high processability, Eu-pcCPG has been utilized as smart ink for secret writing on ordinary paper. Interestingly, the written information appeared only for a few seconds under UV-light and therefore it could be employed for encrypting confidential information. The photo-switchable photophysical properties combined with the high processability of such materials could open exciting opportunities towards developing smart materials for optoelectronics and microscopy applications.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: 10.1039/d0sc05721e |
| This journal is © The Royal Society of Chemistry 2021 |