Effect of Ni/Co mass ratio and NiO–Co3O4 loading on catalytic performance of NiO–Co3O4/Nb2O5–TiO2 for direct synthesis of 2-propylheptanol from n-valeraldehyde

Lili Zhaoab, Hualiang An*a, Xinqiang Zhao*a and Yanji Wanga
aHebei Provincial Key Lab of Green Chemical Technology and High Efficient Energy Saving, Hebei University of Technology, Tianjin 300130, China. E-mail: zhaoxq@hebut.edu.cn; anhl@hebut.edu.cn
bCollege of Science and Technology, Hebei Agricultural University, Huanghua, Hebei 061100, China

Received 19th October 2020 , Accepted 22nd December 2020

First published on 5th January 2021


Abstract

In the direct synthesis of 2-propylheptanol (2-PH) from n-valeraldehyde, a second-metal oxide component Co3O4 was introduced into NiO/Nb2O5–TiO2 catalyst to assist in the reduction of NiO. In order to optimize the catalytic performance of NiO–Co3O4/Nb2O5–TiO2 catalyst, the effects of the Ni/Co mass ratio and NiO–Co3O4 loading were investigated. A series of NiO–Co3O4/Nb2O5–TiO2 catalysts with different Ni/Co mass ratios were prepared by the co-precipitation method and their catalytic performances were evaluated. The result showed that NiO–Co3O4/Nb2O5–TiO2 with a Ni/Co mass ratio of 8/3 demonstrated the best catalytic performance because the number of d-band holes in this catalyst was nearly equal to the number of electrons transferred in hydrogenation reaction. Subsequently, the NiO–Co3O4/Nb2O5–TiO2 catalysts with different Ni/Co mass ratios were characterized by XRD and XPS and the results indicated that both an interaction of Ni with Co and formation of a Ni–Co alloy were the main reasons for the reduction of NiO–Co3O4/Nb2O5–TiO2 catalyst in the reaction process. A higher NiO–Co3O4 loading could increase the catalytic activity but too high a loading resulted in incomplete reduction of NiO–Co3O4 in the reaction process. Thus the NiO–Co3O4/Nb2O5–TiO2 catalyst with a Ni/Co mass ratio of 8/3 and a NiO–Co3O4 loading of 14 wt% showed the best catalytic performance; a 2-PH selectivity of 80.4% was achieved with complete conversion of n-valeraldehyde. Furthermore, the NiO–Co3O4/Nb2O5–TiO2 catalyst showed good stability. This was ascribed to the interaction of Ni with Co, the formation of the Ni–Co alloy and further reservation of both in the process of reuse.


1. Introduction

As an environmentally friendly plasticizer alcohol, 2-propylheptanol (2-PH) can replace 2-ethylhexanol in the production of plasticizers. The industrial process for production of 2-PH comprises a liquid-phase self-condensation of n-valeraldehyde and a subsequent gas-phase hydrogenation of 2-propyl-2-heptenal. The liquid-phase self-condensation of n-valeraldehyde utilizing a dilute NaOH solution as catalyst suffers from several drawbacks such as environmental pollution, apparatus corrosion, and difficulty in recovering and recycling catalyst. The gas-phase hydrogenation of 2-propyl-2-heptenal requires a high energy consumption. If n-valeraldehyde self-condensation and 2-propyl-2-heptenal hydrogenation can be integrated using a multifunctional solid catalyst, that is, direct synthesis of 2-PH from n-valeraldehyde, the industrial production of 2-PH can not only simplify the flow process, but also conform to the requirements for green and sustainable development. Therefore, the multifunctional solid catalyst with high catalytic performance is very important for the reaction integration.

At present, the direct synthesis of 2-PH from n-valeraldehyde was reported over Ru-HT (ruthenium hydrotalcite) bifunctional catalyst but the selectivity of 2-PH was only 48%.1 In a similar reaction integration system, Ni/Ce–Al2O3 showed a better catalytic performance for direct synthesis of 2-ethylhexanol from n-butanal.2 However, the selectivity of 2-ethylhexanol was only 66.9% with a 100% of n-butanal conversion. Additionally, the catalyst suffered from the problem of deactivation due to hydration of γ-Al2O3. It is obvious that improvement of both target product selectivity and catalyst stability is still an unsolved problem.

Titanium dioxide is not only a well-known photocatalyst,3,4 but also can be a good heterogeneous catalyst in the replacement of microporous zeolites and mesoporous (M41S, SBA) materials.5 The KIT-6 incorporating transition metals (Al, Ti, Ce) catalysts with various catalytic applications have high hydrothermal stability compared with the M41S and SBA-15 materials.5–7 In addition, in our previous study on the n-valeraldehyde self-condensation,8 TiO2 showed a high catalytic performance and exhibited a good stability. Moreover, we also evaluated the catalytic performance of Ni/TiO2 for liquid-phase hydrogenation of 2-propyl-2-heptenal and found that Ni/TiO2 had a fairly high hydrogenation performance.9 Based on the above results, we first implemented the one-step synthesis of 2-PH from n-valeraldehyde over Ni/TiO2 catalyst and found that the selectivity of 2-PH was very poor due to a lower competitiveness of n-valeraldehyde self-condensation to n-valeraldehyde hydrogenation. In order to improve the catalytic performance of Ni/TiO2 for n-valeraldehyde self-condensation, Ni/TiO2 was modified by Nb2O5 to tune its acidity and basicity. Therefore, Nb2O5–TiO2 mainly play a catalytic role in the n-valeraldehyde self-condensation. Then the catalytic performance of NiO/Nb2O5–TiO2 catalyst was investigated in order to delay the formation of metal sites on the catalyst surface for further improving the competitiveness of n-valeraldehyde self-condensation reaction. However, NiO was not completely reduced in reaction. To facilitate the complete reduction of NiO in reaction, MOx (M = Pd, Co, Ir or Rh) was introduced into NiO/Nb2O5–TiO2 catalyst to lower the reduction temperature of NiO.10

The key to promotion of 2-PH selectivity in this reaction integration is to enhance competitiveness of n-valeraldehyde self-condensation with respect to direct hydrogenation since the two parallel reactions exist in this reaction system. For this purpose, NiO–Co3O4/Nb2O5–TiO2 was utilized to catalyze the direct synthesis of 2-PH from n-valeraldehyde by means of a reduction-in-reaction operation (reduction of NiO–Co3O4 and n-valeraldehyde self-condensation proceeded simultaneously) in our previous work.9 Therefore, NiO–Co3O4 can be reduced to Ni–Co in the stage of n-valeraldehyde self-condensation reaction, which would play an important role in the successive hydrogenation of self-condensation product or n-valeraldehyde. In this way, n-valeraldehyde self-condensation reaction showed a competitive advantage over its direct hydrogenation since the appearance of metal sites (Ni–Co) was delayed. Therefore selectivity of 2-PH was enhanced while that of n-pentanol was depressed. To further improve the catalytic performance of NiO–Co3O4/Nb2O5–TiO2, effects of Ni/Co mass ratio and NiO–Co3O4 loading were investigated in this work. On this basis, a superior catalytic performance of NiO–Co3O4/Nb2O5–TiO2 was achieved and the reason for its good reusability was analyzed.

2. Experimental

2.1 Catalyst preparation

TiO2 was prepared by a sol–gel method according to the literature8 and Nb2O5–TiO2 was prepared by impregnating TiO2 with an aqueous solution of niobic acid (niobium hydroxide) (dissolving 0.278 g niobic acid (niobium hydroxide) in 50 mL oxalic acid solution (0.5 mol L−1)), followed by aged at room temperature for 12 h, evaporated at 70 °C for 5 h, dried at 120 °C for 12 h and calcination of 450 °C for 2 h.

NiO–Co3O4/Nb2O5–TiO2 catalyst was prepared by co-impregnating Nb2O5–TiO2 with an aqueous solution of Ni(NO3)2·6H2O and Co(NO3)2·6H2O (2.478 g of Ni(NO3)2·6H2O and 0.247 g of Co(NO3)2·6H2O were separately dissolved in 50 mL distilled water), followed by aged at room temperature for 12 h, evaporated at 70 °C for 5 h, dried at 100 °C for 12 h and calcination of 450 °C for 2 h.

NiO/Nb2O5–TiO2 or Co3O4/Nb2O5–TiO2 catalyst was prepared by impregnating Nb2O5–TiO2 with an aqueous solution of Ni(NO3)2·6H2O or Co(NO3)2·6H2O and the remaining steps were similar to the preparation of NiO–Co3O4/Nb2O5–TiO2 catalyst.

2.2 Catalyst characterization

X-ray diffraction (XRD) patterns were measured on a Bruker D8 Advance X-ray diffractometer equipped with a Cu Kα radiation and a graphite monochromator at 100 mA and 40 kV. The scan range covered from 10° to 90° at a rate of 4° min−1.

X-ray photoelectron spectroscopy (XPS) analysis were conducted on a Physical Electronics Kratos Axis Ultra DLD using monochromatic Al Ka X-rays (1486.6 eV) operated at 150 W and 15 kV. The narrow-spectra were obtained with a pass energy of 40 eV and a step increment of 0.100 eV. C 1s peak of 284.6 eV was used as a calibration standard to calibrate the binding energy values.

2.3 Catalyst activity evaluation

30 mL (24 g) of n-valeraldehyde and 3.6 g of NiO–Co3O4/Nb2O5–TiO2 catalyst were placed in a 100 mL stainless steel autoclave and then the air inside was replaced with hydrogen. The mixture was heated to 200 °C and kept for 6 h under a H2 pressure of 3.0 MPa while stirring. After the completion of reaction, the mixture was cooled to room temperature and was separated by centrifugation, and then the liquid was quantitatively analyzed on a SP-2100 gas chromatograph (Beijing Beifen-Ruili Analytical Instrument Co., Ltd) equipped with a flame ionization detector (FID) and a KB-1 capillary column. Cyclohexanol was used as internal standard for improving analytical accuracy.

3. Results and discussion

3.1 Effect of Ni/Co mass ratio

The effect of Ni/Co mass ratio on the catalytic performance of NiO–Co3O4/Nb2O5–TiO2 was investigated and the results are shown in Table 1. It can be seen that all NiO–Co3O4/Nb2O5–TiO2 catalysts showed better performance than NiO/Nb2O5–TiO2 or Co3O4/Nb2O5–TiO2 catalyst. More specifically, the condensation product was not completely hydrogenated over NiO/Nb2O5–TiO2 or Co3O4/Nb2O5–TiO2 catalyst, indicating that a lower hydrogenation activity was ascribed to incomplete reduction of NiO or Co3O4 in the reaction process. However, 2-PH was formed as the main product over NiO–Co3O4/Nb2O5–TiO2 catalysts with different Ni/Co mass ratios. With a decrease of Ni/Co mass ratio, selectivity of 2-PH increased slightly firstly, attained its highest value (81.4%) at a Ni/Co mass ratio of 8/3 and then dropped while that of n-pentanol changed just the opposite.
Table 1 Effect of Ni/Co mass ratio on catalytic performance of NiO–Co3O4/Nb2O5–TiO2 catalysta
Catalyst Ni/Co mass ratio XV/% SPO/% S2-PHEA/% S2-PHA/% S2-PH/%
a Reaction conditions: a weight percentage of catalyst = 15%, T = 200 °C, P = 3 MPa, t = 6 h. X: conversion; S: selectivity. V: n-valeraldehyde; PO: n-pentanol; 2-PHEA: 2-propyl-2-heptenal; 2-PHA: 2-propylheptanal; 2-PH: 2-propylheptanol.b The yield of n-pentanol, 2-propyl-2-heptenal, 2-propylheptanal and 2-propylheptanol was respectively 3.0%, 52.1%, 36.9% and 0%.
NiO/Nb2O5–TiO2b 93.1 3.2 56.0 39.6 0
NiO–Co3O4/Nb2O5–TiO2 10 100 21.8 0 0 77.1
NiO–Co3O4/Nb2O5–TiO2 8/3 100 18.2 0 0 81.4
NiO–Co3O4/Nb2O5–TiO2 6/5 100 34.1 0 0 59.3
NiO–Co3O4/Nb2O5–TiO2 4/7 100 36.7 0 0 56.3
Co3O4/Nb2O5–TiO2 100 20.6 23.1 24.1 13.0


XRD patterns of the fresh and the recovered catalysts of NiO/Nb2O5–TiO2, Co3O4/Nb2O5–TiO2 and NiO–Co3O4/Nb2O5–TiO2 with a Ni/Co mass ratio of 8/3 are shown in Fig. 1. TiO2 anatase crystallite phases were clearly observed in all catalyst samples. The diffraction peaks at 2θ of 37.3° and 43.3° in the fresh NiO/Nb2O5–TiO2 were attributed to (111) and (200) crystal planes of NiO respectively. Similarly, six peaks at 2θ of 19.0°, 31.3°, 36.9°, 44.8°, 59.4° and 65.3° was respectively ascribed to (111), (220), (311), (400), (511) and (440) crystal planes of Co3O4 in the fresh Co3O4/Nb2O5–TiO2.11 Whereas, the peaks of NiO were detected but that of Co3O4 was not found due to a lower Co3O4 loading, a smaller grain size and a higher dispersion on the supporter surface in the fresh NiO–Co3O4/Nb2O5–TiO2 catalyst. For both the recovered NiO/Nb2O5–TiO2 and Co3O4/Nb2O5–TiO2 catalysts, it was obvious that the peaks of NiO or CoO were detected besides metallic Ni or Co, indicating that NiO or Co3O4 was incompletely reduced in the reaction process. However, the peaks of NiO disappeared from the recovered NiO–Co3O4/Nb2O5–TiO2, indicating a complete reduction of NiO in the reaction process possibly due to an interaction of Ni with Co. This may explain the differences in the catalytic performance of the bimetallic oxides and monometallic oxides catalysts as showed in Table 1.


image file: d0ra08903f-f1.tif
Fig. 1 XRD patterns of NiO/Nb2O5–TiO2, Co3O4/Nb2O5–TiO2 and NiO–Co3O4/Nb2O5–TiO2 with a Ni/Co mass ratio of 8/3 before and after reaction. ■: TiO2; ●: NiO; ★: Co3O4; ◆: Ni0; ▲: Co0; ☆: CoO.

In order to further analyze the effect of an interaction of Ni with Co on the catalytic performance of NiO–Co3O4/Nb2O5–TiO2, the recovered NiO–Co3O4/Nb2O5–TiO2 catalysts with different Ni/Co mass ratios were analyzed by XRD and the result is shown in Fig. 2. The characteristic peaks of anatase TiO2 were clearly observed. However, the peaks of NiO and Co3O4 were not detected in all catalyst samples. 2θ value of the corresponding (111) crystal facet was located at between 44.369° of pure metal Co (111) and 44.507° of pure metal Ni (111), indicating that Ni–Co alloy phase was formed during the reaction process.12 Moreover, the diffraction peak of Ni–Co alloy phase (111) crystal plane moved towards the direction of metal Co and gradually approached the characteristic peak of pure metal Co with a decrease of Ni/Co mass ratio. On the contrary, the diffraction peak of Ni–Co alloy phase (111) crystal plane moved towards the direction of metal Ni and gradually approached the characteristic peak of pure metal Ni with an increase of Ni/Co mass ratio.


image file: d0ra08903f-f2.tif
Fig. 2 XRD patterns of the recovered NiO–Co3O4/Nb2O5–TiO2 catalyst with different Ni/Co mass ratios. ■: TiO2; ◆: Ni0; ▲: Co0. (A) XRD patterns; (B) enlarged view of XRD patterns.

The fresh and the recovered catalysts with different Ni/Co mass ratios were analyzed by means of XPS technique. The Ni 2p and Co 2p XPS spectra are shown in Fig. S1 in the ESI. while the measurement data are listed in Tables 2 and 3. Table 2 listed Ni 2p and Co 2p binding energy in the fresh NiO–Co3O4/Nb2O5–TiO2 catalysts with different Ni/Co mass ratios. According to the literatures,13,14 the binding energies at 853.6–853.8 eV and 855.4–855.6 eV are attributed to Ni 2p3/2 peaks of Ni2+, the binding energies at 860.7–861.6 eV and 872.5–873.0 eV are attributed to Ni 2p1/2 peaks of Ni2+, the binding energies at 781.1–781.9 eV and 796.5–797.0 eV are separately attributed to Co 2p3/2 and Co 2p1/2 peaks of Co2+, the binding energies at 779.2–780.4 eV and 794.1–795.8 eV are respectively attributed to Co 2p3/2 and Co 2p1/2 peaks of Co3+. The above results indicate that the mixed metal oxides in the fresh catalyst are NiO and Co3O4. It can be seen from Table 3 that the binding energy at 852.0–852.2 eV is attributed to Ni 2p3/2 peak of Ni0 and the binding energy at 778.1–778.3 eV is attributed to Co 2p3/2 peak of Co0 in the recovered NiO–Co3O4/Nb2O5–TiO2 catalysts.15,16 In addition, the characteristic peaks of NiO and CoO were also be detected due to reoxidation of metallic Ni and Co by contacting air in the analysis process. Moreover, the binding energy of Ni 2p3/2 of Ni0 in the recovered NiO–Co3O4/Nb2O5–TiO2 is lower than that of pure Ni (852.4 eV) while the binding energy of Co 2p3/2 of Co0 is higher than that of pure Co (777.9 eV). This is attributed to the difference in electron work function of Ni and Co.17 Due to a lower electron work function, Co donates electron to Ni, leading to a shift of the binding energies of Ni and Co in Ni–Co alloy.11 This also confirms the interaction of Ni with Co and formation of Ni–Co alloy, in consistence with the result of XRD analysis.

Table 2 Ni 2p and Co 2p XPS data of the fresh NiO–Co3O4/Nb2O5–TiO2 with different Ni/Co mass ratios
Ni/Co Binding energy/eV
Ni2+ Co2+ Co3+
Ni 2p3/2 Ni 2p1/2 Co 2p3/2 Co 2p1/2 Co 2p3/2 Co 2p1/2
10 853.6 861.6 781.9 797.0 780.4 795.0
855.4 872.8
8/3 853.6 860.7 781.2 796.6 779.8 794.8
855.5 872.5
6/5 853.7 861.2 781.1 796.5 779.3 795.8
855.6 872.7
4/7 853.8 861.0 781.1 796.5 779.2 794.1
855.5 873.0


Table 3 Ni 2p and Co 2p XPS data of the recovered NiO–Co3O4/Nb2O5–TiO2 with different Ni/Co mass ratios
Ni/Co Binding energy/eV Number of d-band holes
N0 Co0 Ni2+ Co2+
Ni 2p3/2 Co 2p3/2 Ni 2p3/2 Ni 2p1/2 Co 2p3/2 Co 2p1/2
10 852.2 778.1 853.2 861.7 781.4 797.5 0.77
855.7 872.9
8/3 852.1 778.2 853.8 861.9 781.0 797.0 0.99
855.1 873.0
6/5 852.0 778.3 853.7 861.7 781.0 796.9 1.21
855.7 873.3
4/7 852.0 778.3 853.8 862.2 781.0 796.9 1.43
855.8 873.2


The above analysis results show that the interaction of Ni with Co and formation of Ni–Co alloy make the reduction of NiO easy in the reaction process and NiO–Co3O4/Nb2O5–TiO2 catalyst can be completely reduced to Ni–Co/Nb2O5–TiO2. This result is consistent with that of H2-TPR, H2-TPD, XPS and XRD characterization in our previous study.10 Furthermore, Ni/Co mass ratio has a great effect on the catalytic performance of NiO–Co3O4/Nb2O5–TiO2 catalyst.

To analyze the reason for the best catalytic performance of the catalyst with a Ni/Co mass ratio of 8/3, number of d-band holes of NiO–Co3O4/Nb2O5–TiO2 catalysts with different Ni/Co mass ratios is also listed in Table 3. The energy band theory links the electronic properties of a metal catalyst with its catalysis and d-band holes are used to describe state of valence electron of transition metals. There is a certain relationship among d-band holes of transition metals, adsorption strength of reaction component and the catalytic performance of the transition metal catalyst. Because of an existence of non-paired electrons, the transition metals can interact with reaction component to form chemical bonds. Only when the number of d-band holes in the metal is close to the number of electron transfer in the reaction, can the catalytic performance of the metal be better.18 In hydrogenation reaction, the number of electron transfer of hydrogen molecule adsorbed on metal surface is 1, so the closer to 1 the number of d-band holes of metal catalyst is, the better the catalytic performance. It can be seen from Table 3 that number of d-band holes of the catalyst with a Ni/Co mass ratio of 8/3 is 0.99 (close to 1), so this catalyst should show an excellent catalytic performance, being consistent with the results of catalyst activity evaluation in Table 1.

3.2 Effect of NiO–Co3O4 loading

The effect of NiO–Co3O4 loading on catalytic performance of NiO–Co3O4/Nb2O5–TiO2 with a Ni/Co mass ratio of 8/3 was investigated and the results are shown in Table 4. n-Valeraldehyde could be converted completely with an increase of the loading less than or equal to 17.5 wt%. However, conversion of n-valeraldehyde dropped to 88.0% over a NiO–Co3O4/Nb2O5–TiO2 catalyst with a NiO–Co3O4 loading of 21%, suggesting that the NiO–Co3O4/Nb2O5–TiO2 catalyst with a NiO–Co3O4 loading more than 17.5 wt% may not be reduced completely. The selectivity of 2-PH first increased, reached its highest value over the catalyst with a NiO–Co3O4 loading of 14 wt%, then decreased and finally dropped to zero when NiO–Co3O4 loading was 21 wt%. The selectivity of n-pentanol increased gradually and then decreased. When the loading was 10.5 wt%, the main product was 2-propylheptanal, indicating that the active component of hydrogenation was so less that 2-propylheptanal was not completely hydrogenated to 2-PH. When the loading was higher than 14 wt%, 2-propylheptanal or 2-propyl-2-heptenal was the main product, indicating that NiO and Co3O4 were not completely reduced in reaction due to an over high loading, causing a lower hydrogenation activity.
Table 4 Effect of NiO–Co3O4 loading on catalytic performance of NiO–Co3O4/Nb2O5–TiO2a
Loading of NiO and Co3O4/wt% Loading of NiO/wt% Loading of Co3O4/wt% XV/% SPO/% S2-PHEA/% S2-PHA/% S2-PH/%
a Reaction conditions: a weight percentage of catalyst = 15%, T = 200 °C, P = 3 MPa, t = 6 h. X: conversion; S: selectivity. V: n-valeraldehyde; PO: n-pentanol; 2-PHEA: 2-propyl-2-heptenal; 2-PHA: 2-propylheptanal; 2-PH: 2-propylheptanol.b The yield of n-pentanol, 2-propyl-2-heptenal, 2-propylheptanal and 2-propylheptanol was respectively 4.6%, 66.5%, 15.9% and 0%.
10.5 7.5 3 100 13.4 0 73.2 12.4
14 10 4 100 18.2 0 0 81.4
17.5 12.5 5 100 23.7 0 45.5 28.9
21b 15 6 88.0 5.2 75.6 18.1 0


The XRD patterns of NiO–Co3O4/Nb2O5–TiO2 with different NiO–Co3O4 loading before and after reaction are shown in Fig. 3. When the loading was less than or equal to 14 wt%, the diffraction peaks of NiO were not detected in the recovered catalysts, indicating that NiO could be completely reduced in reaction process. When the loading was higher than 14 wt%, the diffraction peaks of NiO could also be detected besides the diffraction peaks of metal Ni and Ni–Co alloy in the recovered catalysts, indicating that NiO could not be completely reduced in reaction process. The results are consistent with the results of catalyst activity evaluation in Table 4.


image file: d0ra08903f-f3.tif
Fig. 3 XRD patterns of NiO–Co3O4/Nb2O5–TiO2 with different NiO–Co3O4 loading before and after reaction. F: fresh; R: recovered. ●: NiO; ◇: Ni–Co alloy; ◆: Ni0. (A) XRD patterns; (B) enlarged view of XRD patterns.

3.3 Reusability of NiO–Co3O4/Nb2O5–TiO2 catalyst

The NiO–Co3O4/Nb2O5–TiO2 catalyst with a Ni/Co mass ratio of 8/3 and a NiO–Co3O4 loading of 14 wt% was used to evaluate the effect of reaction conditions (see Tables S1–S4 in the ESI) and the suitable reaction conditions were determined as follows: a catalyst amount of 15 wt%, a reaction pressure of 3 MPa, a reaction temperature of 200 °C and a reaction time of 5 h. Under these conditions, the selectivity of 2-PH reached 80.4% at a n-valeraldehyde conversion of 100%.

The recovered NiO–Co3O4/Nb2O5–TiO2 catalyst was washed with ethanol, dried at 120 °C for 6 h, calcinated at 450 °C for 2 h and then was reused in the next cycle. The result of catalyst reusability is shown in Table 5. It can be seen that NiO–Co3O4/Nb2O5–TiO2 catalyst could be reused four times without a significant loss in its catalytic performance. Therefore, NiO–Co3O4/Nb2O5–TiO2 catalyst not only showed a high catalytic performance but also exhibited a good reusability.

Table 5 Reusability of NiO–Co3O4/Nb2O5–TiO2 catalysta
Run XV/% SPO/% S2-PH/%
a Reaction conditions: a weight percentage of catalyst = 15%, P = 3 MPa, T = 200 °C, t = 5 h. V: n-valeraldehyde; PO: n-pentanol; 2-PH: 2-propylheptanol. X: conversion; S: selectivity.
1 100 19.0 80.4
2 100 19.6 80.0
3 100 19.1 80.5
4 100 19.4 80.0
5 100 19.2 80.2


The recovered NiO–Co3O4/Nb2O5–TiO2 catalyst was analyzed by means of XRD technique and the results are given in. Fig. 4. According to literatures19,20 and the PDF cards of JADE5.0 software, the peaks located at 2θ of 44.5°, 51.7° and 76.4° are attributed to pure metal Ni and the peaks located at 2θ of 44.3°, 51.5° and 75.9° are attributed to pure metal Co. It can be seen from Fig. 4 that the peaks located at 2θ of 44.4°, 51.6° and 76.2° can be detected in all the recovered catalysts without calcination (only dried). 2θ = 44.4° of the corresponding (111) crystal facet is located at between 44.3° of pure metal Co (111) crystal facet and 44.5° of pure metal Ni (111) crystal facet, indicating that Ni–Co alloy phase is reserved during the reaction process. This result is in accordance with the XRD analysis in Fig. 2, suggesting that the Ni–Co alloy phase does not change with the reuse of catalyst.


image file: d0ra08903f-f4.tif
Fig. 4 XRD patterns of the recovered NiO–Co3O4/Nb2O5–TiO2. (A) XRD patterns; (B) enlarged view of XRD patterns. ◆: Ni–Co alloy. (a) Recovered from 1st run (only drying); (b) recovered from 2nd run (only drying); (c) recovered from 3rd run (only drying); (d) recovered from 4th run (only drying); (e) recovered from 5th run (only drying).

Takanabe et al.21 found that Co–Ni/TiO2 catalyst with a Ni/Co ratio of 1 showed good catalytic activity and stability due to the formation of Ni–Co alloy. Similarly, Zhang et al.22,23 used Ni–Me (Me = Co, Fe, Cu and Mn) bimetallic catalysts in carbon dioxide reforming of methane and found that Ni–Co bimetallic catalyst exhibited better activity and stability than other bimetallic catalysts due to the synergy between Ni and Co. From the above analysis, a good stability of NiO–Co3O4/Nb2O5–TiO2 should be attributed to the interaction of Ni with Co and formation of Ni–Co alloy in reaction process. Furthermore, both of them could be reserved stably in the process of reuse.

4. Conclusions

NiO–Co3O4/Nb2O5–TiO2 catalyst can be completely reduced to Ni–Co/Nb2O5–TiO2 in reaction process. Its high catalytic performance is ascribed to the interaction of Ni with Co and formation of Ni–Co alloy. The NiO–Co3O4/Nb2O5–TiO2 catalyst with a Ni/Co mass ratio of 8/3 shows the best catalytic performance for its number of d-band holes is nearly equally to the number of electron transfer in hydrogenation reaction. The suitable NiO–Co3O4 loading in NiO–Co3O4/Nb2O5–TiO2 catalyst is 14 wt%. Over high loading results in incomplete reduction of NiO–Co3O4 and then a poor catalytic activity. The selectivity of 2-PH attains 80.4% with a complete conversion of n-valeraldehyde over the NiO–Co3O4/Nb2O5–TiO2 catalyst with a Ni/Co mass ratio of 8/3 and NiO–Co3O4 loading of 14 wt%. Furthermore, the NiO–Co3O4/Nb2O5–TiO2 catalyst can be reused for four times without a decrease in its catalytic activity due to the reservation of the interaction of Ni with Co and formation of Ni–Co alloy.

Conflicts of interest

There are no conflicts of interest to declare.

Acknowledgements

This work was financially supported by National Natural Science Foundation of China (Grant No. 21476058, 21506046, 21978066) and Basic Research Program of Hebei Province for Natural Science Foundation and Key Basic Research Project (18964308D), and Natural Science Foundation of Hebei Province (B2018202220, B2020204023), and the Key Project for Natural Science Foundation of Hebei Province (B2020202048). The authors are gratefully appreciative of their contributions.

References

  1. S. K. Sharma and R. V. Jasra, Indian J. Chem., Sect. A: Inorg., Bio-inorg., Phys., Theor. Anal. Chem., 2005, 54, 451–458 Search PubMed.
  2. N. Liang, X. Zhang, H. An, X. Zhao and Y. Wang, Green Chem., 2015, 17, 2959–2972 RSC.
  3. L. Kumaresan, A. Prabhu, M. Palanichamy and V. Murugesan, Mater. Chem. Phys., 2011, 126, 445–452 CrossRef CAS.
  4. L. Kumaresan, A. Prabhu, M. Palanichamy, E. Arumugam and V. Murugesan, J. Hazard. Mater., 2011, 186, 1183–1192 CrossRef CAS.
  5. A. Prabhu and M. Palanichamy, Microporous Mesoporous Mater., 2013, 168, 126–131 CrossRef CAS.
  6. A. Prabhu, A. Al Shoaibi, C. Srinivasakannan, M. Palanichamy and V. Murugesan, J. Rare Earths, 2013, 31, 477–484 CrossRef CAS.
  7. L. Kumaresan, A. Prabhu, M. Palanichamy and V. Murugesan, J. Taiwan Inst. Chem. Eng., 2010, 41, 670–675 CrossRef CAS.
  8. L. Zhao, H. An, X. Zhao and Y. Wang, Ind. Eng. Chem. Res., 2016, 55, 12326–12333 CrossRef CAS.
  9. L. Zhao, One-step synthesis of 2-propyl heptanol from n-valeraldehyde, Doctoral thesis, Hebei University of Technology, Tianjin, People’s Republic of China, 2019.
  10. L. Zhao, H. An, X. Zhao and Y. Wang, Catal. Commun., 2021, 149, 106209 CrossRef CAS.
  11. L. Zhao, X. Mu, T. Liu and K. Fang, Catal. Sci. Technol., 2018, 8, 2066–2076 RSC.
  12. P. Hu, Z. Y. Chen, T. Chang, J. Deng, F. Yang, K. Wang, Q. Li, B. Hu, H. Yu and W. Wang, J. Alloys Compd., 2017, 727, 332–337 CrossRef CAS.
  13. M. Madkour, Y. K. Abdel-Monem and F. Al Sagheer, Ind. Eng. Chem. Res., 2016, 55, 12733–12741 CrossRef CAS.
  14. J. Li, G. Lu, G. Wu, D. Mao, Y. Guo, Y. Wang and Y. Guo, Catal. Sci. Technol., 2014, 4, 1268–1275 RSC.
  15. L. Xu, F. Wang, M. Chen, J. Zhang, K. Yuan, L. Wang, K. Wu, G. Xu and W. Chen, ChemCatChem, 2016, 8, 2536–2548 CrossRef CAS.
  16. V. S. Kshirsagar, A. C. Garade, K. R. Patil, R. K. Jha and C. V. Rode, Ind. Eng. Chem. Res., 2009, 48, 9423–9427 CrossRef CAS.
  17. F. Yang, N. J. Libretto, M. R. Komarneni, W. Zhou, J. T. Miller, X. Zhu and D. E. Resasco, ACS Catal., 2019, 9, 7791–7800 CrossRef CAS.
  18. J. M. Huo, Carbon dioxide reforming of methane over Ni-Co bimetallic catalyst, Master's thesis, Taiyuan University of Technology, Shanxi, People’s Republic of China, 2015 Search PubMed.
  19. A. W. Burns, A. F. Gaudette and M. E. Bussell, J. Catal., 2008, 260, 262–269 CrossRef CAS.
  20. W. Guo, W. Sun and Y. Wang, ACS Nano, 2015, 9, 1462–11471 Search PubMed.
  21. K. Takanabe, K. Nagaoka, K. Nariai and K. Aika, J. Catal., 2005, 232, 268–275 CrossRef CAS.
  22. J. Zhang, H. Wang and A. K. Dalai, J. Catal., 2007, 249, 300–310 CrossRef CAS.
  23. J. Zhang, H. Wang and A. K. Dalai, Appl. Catal., A, 2008, 339, 121–129 CrossRef CAS.

Footnote

Electronic supplementary information (ESI) available: XPS spectra of NiO–Co3O4/Nb2O5–TiO2 with different Ni/Co mass ratios before and after reaction; catalytic performance of NiO–Co3O4/Nb2O5–TiO2. See DOI: 10.1039/d0ra08903f

This journal is © The Royal Society of Chemistry 2021