Burhannudin
Sutisna
*,
Stoffel D.
Janssens
,
Alessandro
Giussani
,
David
Vázquez-Cortés
and
Eliot
Fried
*
Mathematics, Mechanics, and Materials Unit (MMMU), Okinawa Institute of Science and Technology Graduate University (OIST), 1919-1 Tancha, Onna-son, Kunigami-gun, Okinawa 904-0495, Japan. E-mail: burhannudin.sutisna@oist.jp; eliot.fried@oist.jp
First published on 5th January 2021
Polymer–nanodiamond composites are excellent candidates for the fabrication of multifunctional hybrid materials. They integrate polymer flexibility and exceptional properties of nanodiamonds (NDs), such as biocompatibility, mechanical strength, color centers, and chemically-tailored surfaces. However, their development is hindered by the challenge of ensuring that NDs are homogeneously distributed in the composites. Here, we exploit colloidal coassembly between poly(isoprene-b-styrene-b-2-vinyl pyridine) (ISV) block copolymers (BCPs) and NDs to avoid ND self-agglomeration and direct ND spatial distribution. NDs were first air oxidized at 450 °C to obtain stable dispersions in dimethylacetamide (DMAc). By adding ISV into the dispersions, patchy hybrid micelles were formed due to H-bonds between NDs and ISV. The ISV–ND coassembly in DMAc was then used to fabricate nanocomposite films with a uniform sub-50 nm ND distribution, which has never been previously reported for an ND loading (ϕND) of more than 50 wt%. The films exhibit good transparency due to their well-defined nanostructures and smoothness and also exhibit an improved UV-absorption and hydrophilicity compared to neat ISV. More intriguingly, at a ϕND of 22 wt%, ISV and NDs coassemble into a network-like superstructure with well-aligned ND strings via a dialysis method. Transmission electron microscopy and dynamic light scattering measurements suggest a complex interplay between polymer–polymer, polymer–solvent, polymer–ND, ND–solvent, and ND–ND interactions during the formation of structures. Our work may provide an important foundation for the development of hierarchically ordered nanocomposites based on BCP–ND coassembly, which is beneficial for a wide spectrum of applications from biotechnology to quantum devices.
There has been a growing attention over the past two decades for the development of polymer–nanodiamond composites to create advanced multifunctional materials, owing to the superior mechanical, optical and thermo-electrical properties of nanodiamonds (NDs) as well as their biocompatibility and rich surface chemistry.9,10 NDs are highly relevant in the coating, tribological, and biotech industries11,12 and are frequently used as seeding materials to grow polycrystalline diamond thin films for microdevices.13,14 Morimune et al.15 reported that a small addition of NDs (1 wt%) into poly(vinyl alcohol) (PVA) provided a higher reinforcement compared to that of carbon nanotubes and graphene oxide and increased the Young's modulus by a factor of 2.5 relative to that of neat PVA. The high transparency of the ND-PVA film was also maintained and accompanied by a significant improvement of thermal conductivity. NDs can also improve the performance and stability of supercapacitors when embedded into an electrochemically active polymer of polyanyline.16 More recently, Kulvelis and coworkers17 have also shown that NDs in a prefluorinated membrane used in hydrogen fuel cells can act as a proton reservoir at low temperatures and increase the membrane conductivity at high temperatures. Moreover in biotechnology, polymer–ND composites have shown great potential applications for gene delivery,18 bone scaffold materials,19 post-treatment of root canal therapy,20 and membrane bioreactors.21
Nevertheless, there is still a great challenge in controlling the nanoscopic distribution of NDs in polymeric matrices, as NDs tend to self-aggregate due to the interparticle van der Waals and electrostatic forces.22,23 Previous studies of polymer–ND composites have mainly focused on ND reinforcement properties with lack of nanostructural control, leading to poor nanoscopic distribution and reduced performance at high ND loadings.9,10 Meanwhile, scientists have tailored spatial distribution of various nanoparticles (NPs)24–26 using block copolymers (BCPs), which comprise chains of two or more incompatible macromolecules that self-assemble into ordered mesophases.27 The self-assembly of BCPs in bulk and as colloidal particles with internal morphology can be used to guide gold and silver NPs into hierarchical assembly within the BCP domains.28–30 The extent to which NP size influences their localization within BCP domains has also been discussed.31 BCP-guided NPs can improve reinforcement due to a higher interphase region and possible formation of ordered networks, in contrast to what can be achieved with NP-homopolymer. The nanoscopic arrangement of NPs can also affect optical, magnetic, chemical, electrical, and quantum properties of NPs, which may lead to advanced applications of nanocomposites.32,33 Surprisingly, the use of BCP self-assembly to guide nanoscopic distribution of NDs has rarely been explored. Research on BCP–ND nanocomposites has been limited to ND dispersion stability,34–36 biological applications,37 and elastomeric BCP reinforcements.38,39 Furthermore, in contrast to other spherical NPs, exploring BCP–ND nanocomposites may present a greater challenge due to the self-aggregation behavior of NDs.
In this work, the possibility of controlling the spatial distribution of NDs at the nanoscale is investigated using amphiphilic triblock terpolymers of poly(1,4-isoprene-b-styrene-b-2-vinyl pyridine) (PI-b-PS-b-P2VP). The overview of the materials systems and fabrication methods investigated here is visualized in Fig. 1a. Regular arrangements of NDs on the shells of ISV micelles that are dispersed in dimethylacetamide (DMAc) were obtained by promoting H-bond interactions between NDs and P2VP chains of the terpolymer. Such interactions were established by initially functionalizing NDs with carboxyls through air oxidation. The hybrid micelles can further be used as materials for building transparent and UV-protective films that accommodate well-dispersed NDs at a high ND loading of more than 50 wt%. We also show that ISV and NDs can coassemble into an ordered superstructure with a network-like polymeric matrix and well-aligned ND strings via a step-wise method, which demonstrates the potential ability of directing NDs into arrays over widely separated length scales.
To obtain self-assembled BCP–ND nanocomposites, weighted amounts of ISV terpolymer were dissolved in the previously-prepared ND dispersion in DMAc with a polymer concentration (Cpol) of 10 g L−1. By using different ND concentrations in the dispersion, the ND loading ϕND of the nanocomposites was varied from 22 to 55 wt%. Furthermore, BCP–ND films were fabricated by dropping 30 μL (for thin films) or 90 μL (for thick films) BCP–ND dispersion onto a 1 × 1 cm2 glass substrate, followed by complete solvent-evaporation overnight at an ambient temperature in a fumehood.
Dialysis was performed using 3 mL BCP–ND dispersion (Cpol = 1 g L−1) against 300 mL acetone or ethanol. Proper stirring was applied in the dialysate chamber to maintain a uniform bulk concentration. A solvent-resistant nylon wire was used to hold the enclosed dialysis membrane (bag) ensuring that it remained completely immersed in the dialysate solution without touching the stirrer bar. The system was tightly capped to avoid the dialysate evaporation. The dialysate was changed with a fresh one after overnight dialysis and the operation was continued for several more hours. The dialyzed dispersion was carefully recovered using a syringe and was then stored in a glass vial for further characterizations.
Experimental details on characterization methods are provided in the ESI.†
Raman spectroscopy was then performed (Fig. 1c) to confirm the removal of graphitic carbons during the oxidation process. The measurements were carried out using three different specimens prepared by drop casting and drying DMAc-based suspensions of pristine NDs, NDs annealed at 450 °C, and NDs annealed at 525 °C. The spectra obtained from these specimens were normalized with respect to the graphite G-band peak (≈1600 cm−1); hence, the removal of graphitic carbons is evidenced by the increase in the intensity of the diamond peak (≈1325–1328 cm−1) as the oxidation temperature increases from 450 to 525 °C. The spectra also show that the characteristic disorder-induced double-resonance D-band of NDs peaks at ≈1400 cm−1. Since the Raman cross-section of the sp2 phase is about 50 to 230 times larger than that of diamond,42 the higher intensity of the diamond peak compared to G-band peak after the oxidation clearly shows that the annealing treatment has significantly improved the sp3 phase purity. It is important to recognize that the pristine ND spectra shows some inhomogeneity when measured at different specimen locations in contrast to the oxidized NDs. This suggests that the air oxidation leads to more homogenous distributions of NDs. Although similar spectra as those obtained for 450 °C-oxidized NDs can occasionally be found in pristine ND samples, the pristine ND spectra exhibit a larger shift of the diamond peak (with respect to the single crystal diamond) in comparison to those obtained from oxidized NDs, as shown in Fig. S1a of the ESI.† This shift indicates the presence of tensile strain in the NDs and from the magnitude of the shift we infer that on average the strain gradually reduces as the oxidation temperature increases from 450 to 525 °C.
The XRD spectra presented in Fig. S1b of the ESI† show that all the samples exhibit a diamond (111) Bragg reflection. The peaks are slightly shifted towards smaller 2θ angles with respect to the expected position of unstrained bulk diamond, revealing that the deposited nanodiamonds are characterized by a tensile strain in the range of 0.1–0.2%. In line with the Raman data, the specimen prepared from NDs oxidized at 525 °C displays the smallest shift relative to unstrained bulk diamond and hence the smallest strain. Furthermore, the XRD peak of the sample also features the narrowest full width at half maximum (FWHM), suggesting that annealing at 525 °C also narrows the distribution of lattice constants arising from crystal imperfections and impurities.
Although NDs oxidized at 525 °C exhibit the highest ND purity and O–H content, oxidation at 525 °C results in a significant weight loss, making it less economically viable. We also found that more particles were removed after centrifugation of the sonicated 525 °C-oxidized ND dispersion in DMAc compared to that of 450 °C-oxidized NDs at the same initial concentration and centrifugation conditions. This suggests that larger aggregates were formed by 525 °C-oxidized NDs after sonication in DMAc, presumably affected by an excessive O–H content that prompts additional interparticle H-bonds. As discussed hereinafter, 450 °C was accordingly chosen as the optimum temperature for ND oxidation during the preparation of BCP–ND nanocomposites. The atomic resolution scanning transmission electron microscopy (STEM) image of the ND particles oxidized at 450 °C, depicted in Fig. 1d, shows that a high crystallinity of the annealed NDs is maintained after oxidation. The average size of the crystallites can be estimated from the peak's FWHM of the XRD spectra using the Scherrer formula, suggesting an average size of 4 ± 1 nm, which is consistent with the size of the crystallites shown in the STEM image.
ND dispersions with a Cf of 3–13 g L−1 were mixed with ISV1 at a polymer concentration (Cpol) of 10 g L−1, resulting in ND loading (ϕND) of 22–55 wt% in ISV1–ND nanocomposites (Table S1†). The mixture of ND dispersion at Cf = 17 g L−1 with ISV1 led to precipitation and turbidity and therefore was not used for the investigation. Calculation of the Flory–Huggins interaction parameters (χi,DMAc) presented in Table S2 of the ESI† show that χP2VP,DMAc < χPS,DMAc < χPI,DMAc; thus, while DMAc is a good solvent for P2VP it is a nonsolvent for PS and PI. Hence, ISV1 can be used to form core–shell micelles in DMAc. In these micelles, the PI chains form the micelle core, the core is encapsulated by PS domains, and P2VP corona is located on the outer shell. The pyridine groups of the P2VP corona can therefore interact with the NDs via H-bonds, as illustrated in Fig. 2.
The nanostructures of the ISV1–ND hybrid micelles in DMAc at various ϕND are displayed in Fig. 3. The TEM images show that the NDs form patches on the BCP micelle corona and that this effect becomes more pronounced as ϕND increases. It is noteworthy that the TEM images show aggregates, which presumably formed due to the relatively slow evaporation of DMAc during TEM sample preparation. As the morphology of the hybrid micelles at ϕND values of 22 and 34 wt% can be resolved from the individual micelles that are spotted next to the aggregates. Moreover, since the aggregates mostly feature strings of micelles with NDs on the interfaces between the micelles and at the end of the strings, we infer that the formation of symmetrical patches on the individual micelles is preferred, as illustrated by the schematic. Similarly, at a ϕND of 50 wt%, the micellar constituents of the aggregates are used to interpret the hybrid micelle morphology. To complement the TEM results and analyze the particle size distribution of the hybrid micelles in the dispersions, DLS measurements were performed as discussed hereinafter. The attachment of NDs onto the micelle corona is governed mainly by the H-bond interaction rather than by electrostatic forces, as illustrated in Fig. 2. This is supported by zeta potential measurements, which show that the ISV1 micelles in DMAc have a relatively neutral potential of approximately −4.7 mV, while the oxidized NDs in DMAc exhibit a negatively charged surface of −55.9 ± 3.5 mV. The localization of ND patches on ISV1 micelles at ϕND of 22 and 34 wt% is not yet understood. From the TEM images we infer that the tendency exists for NDs to form patches on two opposing sides of a micelle, as illustrated by the schematic in Fig. 3. However, cases where one or four patches are formed also exist.
DLS analyses of ISV1–ND dispersions are presented in Fig. 3a, c, and e as probability density functions of the particle hydrodynamic radii. At a Cpol of 10 g L−1 (blue-filled curves), the particle sizes increase as ϕND increases, as shown by the shift of average hydrodynamic radii () from approximately 28 nm for ϕND = 22 wt% to approximately 36 nm and 113 nm for ϕND = 34 and 50 wt%, respectively. Additionally, peak broadening indicates an increase in dispersity of the dispersed particles, as driven by an increasing tendency towards particle agglomeration with larger values of ϕND. At Cpol = 10 g L−1 and high ϕND, the interparticle distance appears to be sufficiently close for interparticle ND attraction to cause agglomeration. However, the agglomeration does not spoil the spherical shape of the individual micelles, as can be witnessed from the TEM images. We additionally found that diluting the 10 g L−1 dispersions to 5 g L−1 arrests interparticle agglomeration and leads to the recovery of the individual micelles. The DLS results of the 5 g L−1 dispersions reveal the size recovery of the individual micelles with
= 28 ± 4 nm, consistent with the dimensions of the micellar constituents observed from the TEM images. Since ND coverage of micelles is proportional to ϕND,
at Cpol = 5 g L−1 is found to increase slightly with ϕND.
Our results suggest that patchy hybrid micelles can be fabricated using BCP–ND coassembly via a simple dissolution method. The hybrid micelles may be beneficial as multicompartments for catalyis/biological applications, or can serve as building bricks for designing hierarchically ordered nanocomposites. In this work, we further demonstrate that the hybrid micelles can be utilized to fabricate nanocomposite films with BCP-guided ND distribution. Fig. 4 shows photographs of ISV1–ND films prepared by drop casting the dispersions on glass substrates followed by drying. The pristine ISV1 film (0 wt% NDs) exhibits some opacity caused by light scattering of the film nanostructure and surface roughness. The atomic force microscopy (AFM) depicted in Fig. 4a and b and SEM images depicted in Fig. 5 reveal that elongated structures with sizes of more than 100 nm are formed in the pristine ISV1 film. We hypothesize that these originate from micelle coalescence during solvent evaporation. Also, in the ND containing films, the presence of NDs stabilizes the micelles and preserves the spherical shape of the micelles during the film fabrication. This yields well-defined nanostructures with uniform domain sizes of approximate diameter 50 nm, as estimated from the SEM images, leading to a strong reduction in opacity evidenced from comparing the photographs of the ISV1 and ISV1–ND films. The SEM images in Fig. 5 also show that a uniform distribution of NDs with agglomerate sizes less than 50 nm can be obtained along the film surfaces and cross sections. The ND self-aggregation within the polymer can be significantly reduced, even at a ϕND as high as 55 wt%. However, at ϕND >55 wt%, precipitates were observed in the dispersions and severe cracks appeared in the films. The photographs in Fig. 4 show that the composite films have a brown color, indicating the presence of graphitic phases in the NDs. The reduction of transparency accompanied by these phases can be avoided in the future by using chemical vapor deposition (CVD)-based NDs43 that are highly transparent. Our nanocomposite films can however maintain acceptable levels of transparency at high values of ϕND, an outcome attributable to their nanostructures and the smoothness of their surfaces. As confirmed by the mean square roughness (Sq) and mean roughness (Sa) measurements from 5 × 5 μm2 AFM images that are depicted in Fig. 4b, d, f, and h, the film surfaces become smoother as ϕND increases.
The fabricated films are capable of filtering harmful UV radiation in line with previous reports44,45 on nanodiamond–polymer composite films. These findings were confirmed by UV-Vis spectroscopy measurements yielding data presented in Fig. 6a and b. Although neat ISV1 can absorb UV radiation of wavelength below 280 nm, the addition of NDs can further extend the range of radiation filtering to approximately 400 nm. The spectra also show that the UV protection capacity is proportional to ϕND and the film thickness. This is evidenced by the highest absorption achieved by the thickest ISV1–ND film fabricated in this work with the largest ϕND, namely 44 wt%, as shown in Fig. 6b. The film nearly absorbs 85% of the UV radiation down to a wavelength of 320 nm. The high UV absorption is also accompanied by the film transparency, where around 60–70% of the visible light are transmitted according to the UV-Vis spectra. It is worth notifying that films with a thickness of 13 ± 1 μm, here referred to as thick films, with ϕND > 44 wt% were not characterized due to severe crack formation. The decrease in visible light (340–780 nm) transmittance as ϕND increases is consistent with the visual observation of the films discussed heretofore, which can be attributed to the sp2 inclusions of NDs.
Furthermore, the presence of NDs also improves the surface hydrophilicity, as shown in Fig. 6c. The contact angle θ between a water droplet and film surface decreases with ϕND, which is beneficial for anti-fouling properties in biological applications. To explain this trend qualitatively, we assume that the surface is homogeneously wetted and apply the Cassie equation46
cos![]() ![]() ![]() ![]() | (1) |
cos![]() ![]() ![]() | (2) |
By applying the step-wise method, we find that the copolymer blocks and NDs rearrange simultaneously into a superstructure with a morphology completely different from that of neat ISV1, as evidenced by Fig. 7a–c. To more clearly visualize the suggested superstructures, overfocus TEM images are provided in Fig. S3 of the ESI,† as are lower magnification images. In the absence of NDs, ISV1 self-assembled, in acetone, into a superstructure with a lamellar order. The copolymer chain mobility in acetone is higher since acetone is a good solvent for P2VP and it has a lower Florry–Huggins interaction parameter χij with PS and PI relative to the interaction parameter χij of DMAc with PS/PI (Table S2 of the ESI†). The higher chain mobility of PS and PI in acetone compared to that in DMAc causes the micelles to merge and form a more ordered morphology, namely the lamellar superstructure. It is noteworthy that ordering is also influenced by the molecular weight composition of ISV1. In the presence of NDs, coassembly between ISV1 and NDs occured and resulted in a network-like superstructure at ϕND = 22 wt% as shown in Fig. 7b. However, as ϕND increased to 50 wt% (Fig. 7c), a less-ordered morphology with randomly distributed NDs formed, indicating an order-to-disorder transition at high values of ϕND. Similar phenomena were observed in previous reports describing techniques for using H-bond forming molecules to tailor the morphologies of bulk BCPs52–54 and BCP membranes.55,56 The molecules were found to influence BCP chain stretching and micelle rigidity, or to form subphases that are selectively miscible with one of the copolymer blocks. In our case, NDs containing H-bonding moieties (COOH and OH) are found to affect the ISV1 chain mobility and to form a distinct phase which is selectively miscible with P2VP domains, resulting in morphological transitions of the terpolymer.
![]() | ||
Fig. 7 TEM images of (a) ISV1 terpolymer, (b) ISV1–ND at ϕND = 22 wt%, and (c) ISV1–ND at ϕND = 50 wt% from the dispersions in acetone after dialysis. The dark phases are PI domains stained with OsO4, while ND domains are partially highlighted by dashed red lines. For more clarity, overfocus TEM images are provided in Fig. S3 of the ESI† along with lower magnification images. (d) Particle size distribution of various acetone-dialyzed BCP–ND dispersions after passing through a 5 μm syringe filter: A. ISV1–ND at ϕND = 50 wt%, B. ISV1–ND at ϕND = 55 wt%, C. ISV1–ND at ϕND = 22 wt%, D. ISV2–ND at ϕND = 22 wt%, and E. ISV3–ND at ϕND = 22 wt%. The TEM image insets are the typical aggregates formed in the dispersions. (e) Proposed mechanism of the BCP–ND nanocomposite (22 wt% NDs) superstructure formation upon solvent exchange from DMAc to acetone. The schematic illustration elucidates how the oxidized NDs attached on the P2VP corona (red color) arrange into strings guided by the BCP self-assembly. The presence of acetone increases the mobility of PS (gray color), which leads the micelle corona to merge and the soft PI core (blue color) to coalesce. As the dispersion is richer with acetone, the BCP–ND coassembles to a 3D network with well-organized interconnected ND strings. |
We emphasize that the dialysis against acetone resulted in the formation of turbid supernatant accompanied by some precipitates. The TEM images depicted in Fig. 7a–c represent local observations of precipitate morphology. Concurrently, the particles that are dispersed in the supernatant, further called aggregates, exhibit a morphology similar to that of the precipitates with average particle diameters between 100–300 nm, as discussed hereinafter. The formation micron scale precipitates with uniform internal morphology indicates that the generated superstructures exhibit a long-range order. Additionally, it implies that the BCP–ND coassembly can be directed to form arrayed nanostructures over manifold length scales, which is essential for the fabrication of functional devices.
Since both the precipitates and the suspended aggregates have the same internal morphology, we assume that the precipitates were formed kinetically from the aggregates as their concentration increases during the dialysis process. To better understand the colloidal coassembly of ISV1–ND during the dialysis process, the supernatants were analyzed using DLS after filtering the dialyzed ISV1–ND dispersions through 5 μm pore-size polytetrafluoroethylene (PTFE) syringe filters. The DLS results displayed in Fig. 7d show that the ISV1–ND dispersion with ϕND = 22 wt% (curve C) comprises larger aggregates than those obtained for higher values of ϕND (curves A and B). This finding is supported by the TEM image insets of curves A and C, which display the morphology of aggregates formed in the corresponding dispersions. This phenomenon can be related to the influence of NDs on polymer chain mobility, as discussed below.
A sufficiently high ϕND (50 and 55 wt%) stabilizes the BCP micelles in the dispersion and obstructs the copolymer chain mobility to further coalesce and coassemble into a larger aggregate as in the case of ϕND = 22 wt% and, hence, to form smaller aggregates. Fig. 7d also shows that aggregates from ISV1–ND with ϕND = 55 wt% (curve B) are larger than those obtained for ϕND = 50 wt% (curve A); this is because the initial micelle size and ND–ND interactions increase with ϕND. At ϕND = 22 wt%, larger aggregates with an ordered morphology were formed, indicating that, at such ND loading, chain mobility is sufficient to allow micelles to merge and self-assemble into a superstructure with cylindrical PI cores in an interconnected PS matrix, while the P2VP domain stabilizes the NDs at the interfaces. Accordingly, NDs that are attached onto the P2VP chains by H-bonds assemble into interconnected strings, as illustrated in Fig. 7e.
At ϕND = 22 wt%, similar morphologies (shown in Fig. S3 of the ESI†) were also attained using ISV terpolymers with different molecular weight compositions, namely ISV2 and ISV3 (see Table 1). The DLS measurements of ISV2–ND and ISV3–ND dispersions in acetone (curves D and E of Fig. 7d, respectively) reveal the formation of smaller aggregates compared to that of ISV1–ND. This result can be explained by analysing the molar volume ratio of P2VP to PS (VP2VP/VPS) in the corresponding ISV terpolymers. The molar volume of block i was calculated by dividing its molecular weight by its mass density ρi, with ρPS = 1.04 kg L−1and ρP2VP = 1.14 kg L−1.57 We find that as VP2VP/VPS decreases from ISV1 to ISV3 (ISV1 = 0.21, ISV2 = 0.20, and ISV3 = 0.17), the average hydrodynamic radii of the aggregates decrease. The compositional analysis shows P2VP and PS are more compatible with acetone than is PI. This implies that P2VP and PS dominate the copolymer chain mobility during the formation of aggregates. Moreover, of the polymer block components we considered, P2VP is the most soluble in acetone, and the attachment of NDs on P2VP further increases its influence on aggregate formation due to the interparticle ND attraction. We accordingly infer from the experimental results that with higher P2VP to PS ratios the tendency to form larger aggregates is enhanced.
The strong influence of NDs in the formation of agglomerates during ISV1–ND coassembly was also corroborated by dialyzing neat ISV1 and ISV1–ND dispersions in DMAc against ethanol (EtOH). TEM and DLS measurements of neat ISV1 dialyzed against EtOH (Fig. S5a and S5c†) suggest that a stable and monodispersed ISV1 dispersion in EtOH with of 29 nm was obtained without spoiling the core–shell morphology of the micelles. Since EtOH is a good solvent for P2VP and a nonsolvent for PS and PI (Table S1†), the P2VP corona can stabilize neat ISV1 core–shell micelles and micelle agglomeration is avoided when changing the solvent from DMAc to EtOH. On the other hand, due to the gluing effect of NDs, the ISV1–ND micelles tend to agglomerate, without changes to their individual micellar shape, after exchanging the solvent from DMAc to EtOH (Fig. S5b and S5c†). The formation of agglomerates might be affected by the intermicelle-ND attraction, which is more favorable in EtOH due to the lower polarity index of EtOH (P′EtOH = 4.3) relative to that of DMAc (P′DMAc = 6.5).58
In summary, our experimental results suggest a complex interplay between BCP self-assembly in solutions, BCP–ND interactions, and ND colloidal behaviors. Whereas a proper interaction between BCPs and a selective solvent is required to generate a desired BCP self-assembled morphology, a preferential compatibility between NDs and BCPs is also crucial to achieving thermodynamically stable ordered structures with well dispersed NDs. The presence of preferential H-bond interactions between BCPs and NDs revealed in this work qualitatively demonstrates the importance of minimizing the enthalpy of mixing between BCP and NDs. Furthermore, our experimental results show the influence of ND loading ϕND on the polymer chain mobility, which suggests a similar behavior to the incorporation of NPs into BCPs in bulk, that involves polymer-chain conformational entropy and translational entropy of NPs.59,60 Our findings also suggest that ND self-agglomeration further complicates not only the thermodynamics but also the kinetics of BCP–ND coassembly. On the thermodynamic side, this might give rises to a free energy penalty by ND–ND interactions qualitatively similar to energetic contributions due to rod–rod interactions in BCP-nanorod blends investigated by Thorkelsson and co-workers.61 On the kinetic side, ND self-agglomeration that occurs for sufficiently high values of ϕND might increase the activation energy barrier for interdomain diffusion and thereby impede long-range diffusion, as observed for high loadings of AuNPs in supramolecular nanocomposites reported by Kao et al.62 Additionally, apart from the fact that BCP self-assembly can guide ND arrays, the formation of ND strings observed in our experiments, either in the patchy hybrid micelles or in the self-assembled superstructures, may point to a tendency for NDs to self-assemble in solution. This resonates with a recent report by Chang et al.63 concerning the dynamic self-assembly of NDs in water that can form strings due to electrostatic forces, chemical functionalities, and surrounding medium. Such colloidal behavior of NDs may contribute to an entropic factor related to the aggregate orientation as described previously for NP localization in BCP micelles.64
Secondly, our patchy hybrid micelles also exhibit potential utility as objects for building self-assembled superstructures and hybrid multicompartment micelles (aggregates) with well-organized ND arrays via a step-wise dialysis method against acetone. The BCP–ND nanocomposites with an ND loading of 22 wt% were found to possess a fascinating network-like morphology which exhibits long-range order. The structure features interconnected ND strings within a self-assembled polymeric matrix as hybrid multicompartment micelles and self-assembled superstructures. This result also underscores the possibility of controlling nanoscale ND arrangement in polymeric nanocomposites, which has never been previously investigated. The formation mechanism of the reported structures was studied by performing TEM and DLS analyses which testify to the indispensable roles of polymer–polymer, polymer–solvent, polymer–ND, ND–solvent, and ND–ND interactions in determining the nanocomposite morphology. Our work may lead to a scalable bottom-up strategy for guiding ND assembly into arrays. Such a strategy would benefit a wide spectrum of applications in biotechnology, high performance coating, energy harvesting and storage, and quantum devices.
Despite the complexity of BCP–ND colloidal coassembly, we suppose that wet-based techniques are preferable to dry alternatives like extrusion and milling since they can improve polymer chain mobility and reduce ND self-agglomeration by solvation. Further study is, however, needed to discover pathways to different possible combinations of ND surface chemical modifications, polymer functionalities, solvent polarity, and fabrication routes. Owing to the biocompatibility of NDs, it might also be interesting to investigate methods for forming multicompartment nanostructures68,69 based on BCP and NDs. Since BCPs have been recognized as synthetic materials that can be used to construct models for biological systems,70,71 our findings may also provide a foundation for advanced bio-applications of NDs. Furthermore, a systematic theoretical study of BCP–ND coassembly in solution is also highly desired to better understand the kinetics of structure formation, predict other possible thermodynamically stable structures, and obtain optimum conditions for achieving targeted material properties.
In addition, since assembling NDs into arrays is crucial for their applications in quantum sensings72,73 and quantum information processings,74 our work may open a new avenue for directing arrays of NDs with quantum properties. Previous works have been performed to direct fluorescent ND assembly including the use of lithography techniques,75,76 or biological molecules.77,78 However, to the best of our knowledge, our approach is an unprecedented strategy to guide ND nanoscopic arrangement by using BCP self-assembly, which can be more scalable for designing quantum devices.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/D0NR07441A |