Open Access Article
This Open Access Article is licensed under a
Creative Commons Attribution 3.0 Unported Licence

Enhanced thermoelectric properties exhibited by unreduced freestanding graphene oxide/carbon nanotube membranes

Md. Saidul Islam ab, Hitomi Ohmagari ac, Mohammad Atiqur Rahman a, Yuta Shudo a, Masahiro Fukuda a, Junya Yagyu a, Yoshihiro Sekine ad, Leonard F. Lindoy e and Shinya Hayami *ab
aDepartment of Chemistry, Faculty of Advanced Science and Technology, Kumamoto University, 2-39-1 Kurokami, Kumamoto 860-8555, Japan. E-mail: hayami@kumamoto-u.ac.jp
bInstitute of Industrial Nanomaterials (IINa), Kumamoto University, 2-39-1 Kurokami, Kumamoto 860-8555, Japan
cCollege of Science and Engineering, Aoyama Gakuin University, 5-10-1 Fuchinobe, Chuo-ku, Sagamihara, Kanagawa 252-5258, Japan
dPriority Organization for Innovation and Excellence, Kumamoto University, 2-39-1 Kurokami, Chuo-ku, Kumamoto 860-8555, Japan
eSchool of Chemistry F11, The University of Sydney, Sydney, New South Wales, 2006, Australia

Received 1st April 2021 , Accepted 11th June 2021

First published on 11th June 2021


Abstract

Herein we determine the Seebeck coefficients, electric conductivities, and thermoelectric power factors of a range of unreduced graphene oxide (GO)/single-wall carbon nanotube (CNT) membranes incorporating different GO/CNT ratios as well as of a series of reduced graphene oxide (rGO) membranes for which reduction had occurred at different temperatures. The considerable thermoelectric power factor of 5.33 × 10−2 μW mK−2 generated from unreduced GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]2 ratio) is in agreement with its suitability for application as a flexible thermoelectric material. Moreover, compared to the conventional architectures of traditional thermoelectric materials, the inherent flexibility of GO-based thermoelectric materials opens the door to improved performance and efficiency, with lightweight, scalable, stretchable, and/or wearable materials being the outcome.


1. Introduction

The thermoelectric phenomenon is considered as a green technique to produce electrical energy using the thermal electromotive force induced due to a temperature difference between two ends of a thermoelectric material, where charge carriers diffuse across the temperature gradient. This results in a build-up of charge and thus creates a potential difference.1–4 Thermoelectric devices are all-solid-state devices with no moving parts and thus can be employed without generating noise or other pollution. Even though the energy efficiency from thermoelectric process is quite small, the widespread use of low-temperature driven thermoelectric energy conversion devices could be useful for producing electricity anywhere by utilizing the heat from sunlight, the waste heat from different systems or even from the human body. So far, the best thermoelectric materials are inorganic compounds (such as Bi2Te3) that have relatively low earth abundance and are fabricated through highly complex vacuum processing routes that limit their full potential for widespread use. Consequentially, the development of alternative efficient, cheap, and abundant thermoelectric materials represents the key to the future advancement and large scale commercialization of thermoelectric devices.4–7 The suitability of a thermoelectric material is determined by the device efficiency which is related to the thermoelectric figure of merit zT, given by zT = σS2T/k where σ S, T, and k represent the material's electrical conductivity, Seebeck coefficient, temperature, and thermal conductivity, respectively. The term σS2 corresponding to the power factor of a thermoelectric material, plays a significant role in determining its efficiency.8–10

Compared to 3D bulk materials, decreasing the dimension of a thermoelectric compound towards a 2D structure is expected to result in better thermoelectric properties, including higher electrical conductivity coupled with lower thermal conductivity as a consequence of the discretization of the electric state density, the construction of interfaces between the layered compound, and the quantum confinement effect.11–14 In addition, compared to the conventional bulky 3D geometrical architectures of traditional thermoelectric materials, the flexibility in the design of such 2D materials open the possibility for improving performance and giving rise to lightweight, scalable, stretchable, and wearable properties.15–17 The unique properties of graphene oxide (GO) sheets along with the uniform layered stacking arrangement with sufficient mechanical strength to act as a free-standing membrane is a distinctive advantage making GO attractive for thermoelectric application. Unlike graphene with its high thermal conductivity which limits its suitability for practical thermoelectric applications (despite a considerable Seebeck coefficient and high electrical conductivity), density functional theory (DFT) results indicate that adding oxygen into the graphene lattice (i.e., to produce GO) significantly reduces its thermal conductivity due to the phonon scattering effect resulting from both acoustic mismatch and reduced symmetry in the graphene structure; hence GO appears a promising candidate for constructing thermoelectric materials.18,19 Nevertheless, pristine GO is associated with low electric conductivity and this is identified as the key concern for its practical use in GO-based thermoelectric materials. Previous studies on GO-based thermoelectric materials have focused on reduced graphene oxide (rGO) for improving the electrical conductivity while the restoration of some sp2 hybridized C atoms has been shown to be responsible for improved electrical conductivity.20–23 Unfortunately, the Seebeck coefficient is sharply decreased with a high degree of rGO reduction, with the expectation that thermal conductivity will increase due to the graphene-like structure of rGO. Even though, the GO-based hybrid prepared by adding carbon nanotubes (CNT) to the GO has been reported to increase in thermal conductivity which was attributed to the formation of 3D heat conduction paths by the addition of MWCNTs.24 However, the thermal conductivity of GO/CNT is expected to the less than that of pristine CNT or rGO and might be facilitated the thermoelectric properties of GO/CNT hybrid.

Thus, in the present work we consider the prospect of employing unreduced GO for use in thermoelectric materials. The electrical conductivity of unreduced GO membrane was increased by the introduction of single wall CNT in different ratios while keeping the functional groups of the GO intact. In addition, we also investigated the effect of the temperature used for the reduction of GO (annealed at different temperatures ranging from 100 to 400 °C) on the corresponding thermoelectric behaviour. The Seebeck coefficients and electrical conductivities have been measured and the corresponding thermoelectric power factors (σS2) calculated. The maximum thermoelectric potential and Seebeck coefficient were observed for rGO whose reduction occurred at 100 °C. However, the highest electric conductivity and thermoelectric power factor were obtained from the sample composed of a 1[thin space (1/6-em)]:[thin space (1/6-em)]2 ratio of GO/CNT.

2. Experimental

GO dispersion in water was purchased from Nippon Shokubai Co., Ltd. CNT was obtained from Sigma Aldrich. The GO film was prepared from the GO dispersion (1 mg/5 mL) employing a membrane filter with a pore size of 0.4 μm, followed by drying the product film under ambient conditions. Thermal annealing at the desired temperature was employed to prepare the rGO samples. The products from reduction at 100, 120, 140, 160, 300, 400 °C were designated as rGO@100–rGO@400, respectively. Unreduced GO and CNT dispersion were mixed in the ratios (by weight) 1[thin space (1/6-em)]:[thin space (1/6-em)]0.5, 1[thin space (1/6-em)]:[thin space (1/6-em)]1 and 1[thin space (1/6-em)]:[thin space (1/6-em)]2 and denoted as GO/CNT(1[thin space (1/6-em)]:[thin space (1/6-em)]0.5), GO/CNT(1[thin space (1/6-em)]:[thin space (1/6-em)]1), and GO/CNT(1[thin space (1/6-em)]:[thin space (1/6-em)]2), respectively. The mixed suspensions were each filtered through a membrane using reduced pressure to obtain freestanding GO/CNT membranes.

The structure and morphology of the samples were characterized by field emission scanning electron microscopy (FE-SEM, JSM-7600F, JEOL), Fourier transform infrared spectroscopy (FT-IR, Spectrum Two, PerkinElmer) and X-ray diffraction spectroscopy. Seebeck coefficients for the respective samples involved measuring the temperature differences between opposing ends of individual samples. The dimension including length, width and thickness of each sample were 1.8 cm, 0.5 cm and ∼30 μm, respectively. One end is contacted with a peltier element connected to a power supply (hot end) while the opposite end was maintained at ambient temperature (cold end) to create a temperature difference between these ends as shown in Fig. S1 (ESI). The temperature difference was maintained at 36 K. The thermo-voltage generated between the two ends was measured using a PC510 digital multimeter by attaching silver-pasted thin copper wire probes in contact with each end.

3. Results and discussion

The SEM images (Fig. 1a and b) show the cross-sectional morphology of the GO and GO/CNTs (1[thin space (1/6-em)]:[thin space (1/6-em)]2) membranes, respectively. Clearly, GO shows a characteristic layer by layer membrane morphology. For the GO/CNT membrane, the CNT is found to be well dispersed in a compact arrangement in the resulting freestanding membrane.
image file: d1ma00299f-f1.tif
Fig. 1 Cross sectional SEM images. (a) GO and (b) GO/CNT with 1[thin space (1/6-em)]:[thin space (1/6-em)]2 weight ratio. (c) PXRD patterns for GO and rGO at 100 to 180 °C; (d) FTIR spectra for GO and rGO at 100 to 180 °C.

The SEM images of GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]0.5) and GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]1) are given in Fig. S2 (ESI). Upon reduction of GO membrane at higher temperatures (100 to 400 °C), the interlayer distance for GO is decreased and this was also confirmed by PXRD. The PXPD patterns for GO and rGO measured after reduction at temperatures ranging from 100 to 160 °C are presented in Fig. 1c. The characteristic PXRD peak for GO (002) at 2θ = 10.48° shifts to the higher angles of 11.15°, 11.94°, 22.50° and 22.90° for rGO@100, rGO@120, rGO@140, and rGO@160, respectively. The calculated interlayer distances for GO, rGO@100, rGO@120, rGO@140, rGO@160 are 8.44 Å, 7.94 Å, 7.41 Å, 3.95 Å, and 3.88 Å, respectively. The decrease in the interlayer distances can be attributed to both the removal of the adsorbed water as well as to decomposition of some of the oxygen functional groups.

The XRD patterns for rGO@300 and rGO@400 are shown in Fig. S3 (ESI). The respective broad peaks at 24.04° and 24.58°, indicate that the (002) plane has shifted towards higher angles, with the corresponding interlayer distances being 3.70 Å and 3.62 Å, respectively. The interlayer distance is drastically decreased from rGO@120 (7.41 Å) to rGO@140 (3.95 Å) indicating that a large number of oxygen-containing functional groups in GO were removed at 140 °C. The FT-IR spectra of rGO@100, rGO@120, rGO@140, rGO@160 as well as of GO were obtained (Fig. 1d). Compared to the peaks associated with the epoxy groups (c. 1080 cm−1) and hydroxyl groups (c. 3400 cm−1) in the spectrum of rGO@120, the change in these peak intensities observed for rGO@140 is in accord with a reduction of the epoxy and hydroxyl groups present having occurred in the latter case.

The thermo-voltages measured across the opposite ends of the different “weight ratio” samples (temperature difference 36 K) are presented in Fig. S4 (ESI). The maximum voltage (of 1.76 mV) was observed for rGO@100, with the magnitude of voltage decreasing sharply with increase in reduction temperature. The thermo-voltages obtained for GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]0.5), GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]1), and GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]2), are 0.0332, 0.0445, and 0.0326 mV, respectively. The corresponding Seebeck coefficients are presented in Fig. 2a and Table 1. An exceptionally high Seebeck coefficient of 1350 μV K−1 was obtained for rGO@100. However, the reduction of GO at elevated temperature significantly decreases the Seebeck coefficient value. For example, the Seebeck coefficient for rGO@400 is only 6.7 μV K−1 while, on the other hand, the value for GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]1) is 44.5 μV K−1. Lower and higher ratios of GO[thin space (1/6-em)]:[thin space (1/6-em)]CNT were both observed to result in somewhat lower Seebeck coefficients. For example, the values for GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]0.5) and GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]2) are 32.0 and 28.6 μV K−1, respectively.


image file: d1ma00299f-f2.tif
Fig. 2 Thermoelectric properties of GO-hybrids. (a) Seebeck coefficients for GO, rGO(100–400 °C) and GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]0.5, 1[thin space (1/6-em)]:[thin space (1/6-em)]1, and 1[thin space (1/6-em)]:[thin space (1/6-em)]2 weight ratios); (b) electrical conductivities and thermoelectric power factors for GO, rGO (100–400 °C), and GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]0.5, 1[thin space (1/6-em)]:[thin space (1/6-em)]1, and 1[thin space (1/6-em)]:[thin space (1/6-em)]2).
Table 1 Thermoelectric properties of the prepared GO-based hybrid membranes
Sample name Seebeck coefficient conductivity(μV K−1) Electrical conductivity (S cm−1) Power factor (μW mK−2)
GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]0.5) 32.0 9.85E-03 1.01E-03
GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]1) 44.5 2.23E-02 4.41E-03
GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]2) 28.6 6.52E-01 5.33E-02
GO 432 5.96E-08 1.11E-06
rGO@100 1350 1.77E-06 3.22E-04
rGO@120 34.4 1.26E-03 1.49E-04
rGO@140 1.25 7.33E-03 1.14E-06
rGO@160 4.07 1.44E-02 2.23E-05
rGO@300 5.8 1.35E-02 5.55E-05
rGO@400 6.7 3.44E-02 1.57E-04


The electrical conductivities of the samples measured under their respective “temperature-difference” conditions are presented in Fig. 2b and Table 1. The electric conductivities of GO and rGO@100 are both very low but the values increase significantly for the other (higher-temperature reduction) samples. The electrical conductivities increase from 5.98 × 10−8 S cm−1 for GO to 3.44 × 10−2 S cm−1 for rGO@400. Interestingly the electric conductivity of GO/CNT is much higher than even rGO@400. Moreover, the value increases with an increasing proportion of CNT in the GO/CNT sample. The highest electric conductivity of 6.52 × 10−1 S cm−1 was achieved for GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]2).

Finally, the power factors for all membrane samples were calculated using power factor = σ × S2 and are presented in Fig. 2b and Table 1.

The maximum power factor obtained for the samples prepared is 5.33 × 10−2 μW mK−2 for the GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]2) product. The power factors for GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]0.5) and GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]1) are 1.01 × 10−3 and 4.41 × 10−3 μW mK−2, respectively. Pristine GO shows a very low power factor of 1.11 × 10−6 μW mK−2. For the rGO samples, rGO@100 shows the maximum power factor of 3.22 × 10−4 μW mK−2 (Table 1).

As an extension of the above, we have employed body heat (finger contact) as the heat source to exploit the Seebeck effect in a rGO@100 film. In this case a temperature difference of 12 K (versus ambient) was achieved. The excellent reversible behaviour following alternate finger contact/non-contact against time is shown In Fig. 3.


image file: d1ma00299f-f3.tif
Fig. 3 Thermoelectric response of rGO@100 membrane with temperature difference employed form body heat (temperature difference 12 K).

In general, the Seebeck coefficient and the electrical conductivity of materials depend on the charge carrier concentration; with an inverse relationship existing between them.25 Thus, semiconductors/insulators have large Seebeck coefficients and hence low electrical conductivities. GO and GO@100 have very low carrier concentrations, reflecting the presence of the oxygen-containing functional groups, and hence high Seebeck coefficients and very low electronic conductivity. Compared to the pristine GO, the rGO@100 showed the higher Seebeck coefficient value which might be attributed to the removal of the water molecules. In principle, the adsorbed water molecules are removed from the GO during calcination at 100 °C.26 Upon reduction at elevated temperatures, the oxygen-functionalized groups are decomposed (Fig. 1c and d) leading to the restoration of sp2-carbons in the membrane structure and resulting in higher carrier concentrations with a concomitant increase in the electrical conductivity (and accompanied by a decrease in the Seebeck coefficient).25

The required properties of an ideal thermoelectric material include (i) an adequate Seebeck coefficient (ii) high electrical conductivity, and (iii) low thermal conductivity. As for graphene, the thermoelectric properties of pristine CNT are limited due to its high thermal conductivity.27 In the current study, the synergism arising from employing both these to produce hybrid unreduced GO/CNT membranes has resulted in enhanced thermoelectric properties where CNT contributes to the high electrical conductivity while GO contributes the presence of an adequate Seebeck coefficient. As a consequence, the unreduced GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]2) membrane showed a high thermoelectric power factor of 5.33 × 10−2 μW mK−2. Previously there have some reports on rGO and rGO based composites as efficient thermoelectric materials.28–31 For example, Mehmood et al. reported the thermoelectric power factor of 2.21 × 10−3 μW K−2 m−1 for flat rGO film.28 The power factor of ∼0.93 μW K−2 m−1 for rGO films obtained from 4 h hydrothermal reactions and deposited on a glass substrate.29 In another study, the power factor value of ∼0.43 μW K−2 m−1 was reported for rGO with PANI composite material obtained by spark plasma sintering (rGO[thin space (1/6-em)]:[thin space (1/6-em)]PANI as 30[thin space (1/6-em)]:[thin space (1/6-em)]70).30 In addition, the value of pure rGO paper were calculated as ∼3.0 × 10−2 μW K−2 m−1 which then increase to 1.2 μW mK−2 using rGO + 50%CNT paper.31 However, the current work is the first report for free-standing unreduced GO/CNT as thermoelectric materials with a comparable power factor of 5.22 × 10−2 μW K−2 m−1. Unfortunately, the estimation of the thermal conductivity of our GO/CNT membrane is beyond our current scope. However, some recent studies report the much lower thermal conduction (more than 90%) of graphene oxide compared to graphene.18,19 The oxygen-containing functional groups reduce the efficiency of phonon transport in graphene oxide and adversely affect the thermal performance due to the mean free path of phonons being limited mainly by interior defects resulting from both acoustic mismatch and reduced symmetry in the graphene structure.18,19 Arising from this, the resulting unreduced GO/CNT composite is expected to exhibit low thermal conductivity and hence shows much promise for low-temperature driven thermoelectric devices in the future.

4. Conclusions

In conclusion, we have successfully prepared freestanding hybrid membranes using unreduced GO and CNT in different ratios which show enhanced thermoelectric properties. In particular, the GO/CNT (1[thin space (1/6-em)]:[thin space (1/6-em)]2) membrane exhibited a significant enhancement in terms of the Seebeck coefficient, electric conductivity, and thermoelectric power factor with values of 28.6 μV K−1, 6.52 × 10−1 S cm−1, and 5.33 × 10−2 μW mK−2, respectively. On the other hand, despite rGO@100 showing a very high Seebeck coefficient, the low electric conductivity reduces its thermoelectric power factor and, consequently, also its suitability for practical application. In addition, at higher reduction temperatures (i.e., that employed to obtain rGO@400), the Seebeck coefficient was sharply reduced resulting in a low power factor. The current study signifies that pristine GO or rGO appear less than ideal for use as thermoelectric materials for practical application. Instead, unreduced GO with electron conductive additives (in the present study CNT) appears a promising pathway towards efficient thermoelectric materials. We propose that the results from the current study will provide a basis for important future developments in the area.

Conflicts of interest

There are no conflicts to declare.

Notes and references

  1. Z. Soleimanim, S. Zoras, B. Ceranic, S. Shahzad and Y. Cui, Sustainable Energy Technol. Assess., 2020, 37, 100604 Search PubMed.
  2. P. Ren, Y. Liu, J. He, T. Lv, J. Gao and G. Xu, Inorg. Chem. Front., 2018, 5, 2380 Search PubMed.
  3. S. Twaha, J. Zhu, Y. Yan and B. Li, Renewable Sustainable Energy Rev., 2016, 65, 698 Search PubMed.
  4. B. Poudel, Q. Hao, Y. Ma1, Y. Lan, A. Minnich, B. Yu, X. Yan, D. Wang, A. Muto, D. Vashaee, X. Chen, J. Liu, M. S. Dresselhaus, G. Chen and Z. Ren, Science, 2008, 320, 634–638 Search PubMed.
  5. R. Venkatasubramanian, E. Siivola, T. Colpitts and B. O’Quinn, Nature, 2001, 413, 597–602 Search PubMed.
  6. H. J. Goldsmid, Proc. Phys. Soc., London, 1958, 71, 633 Search PubMed.
  7. B. Russ, A. Glaudell, J. J. Urban, M. L. Chabinyc and R. A. Segalman, Nat. Rev. Mater., 2016, 1, 16050 Search PubMed.
  8. W. Liu, H. S. Kim, Q. Jie and Z. Ren, Scr. Mater., 2016, 111, 3–9 Search PubMed.
  9. T. Mori, Small, 2017, 13, 1702013 Search PubMed.
  10. I. Petsagkourakis, K. Tybrandt, X. Crispin, I. Ohkubo, N. Satoh and T. Mori, Sci. Technol. Adv. Mater., 2018, 19, 836 Search PubMed.
  11. L. D. Hicks and M. S. Dresselhaus, Phys. Rev. B: Condens. Matter Mater. Phys., 1993, 47, 12727 Search PubMed.
  12. K. Takahata, Y. Iguchi, D. Tanaka, T. Itoh and I. Terasaki, Phys. Rev. B: Condens. Matter Mater. Phys., 2000, 61, 12551 Search PubMed.
  13. Y. Mizuguchi, H. Fujihisa, Y. Gotoh, K. Suzuki, H. Usui, K. Kuroki, S. Demura, Y. Takano, H. Izawa and O. Miura, Phys. Rev. B: Condens. Matter Mater. Phys., 2012, 86, 220510 Search PubMed.
  14. Y. Mizuguchi, S. Demura, K. Deguchi, Y. Takano, H. Fujihisa, Y. Gotoh, H. Izawa and O. Miura, J. Phys. Soc. Jpn., 2012, 81, 114725 Search PubMed.
  15. Y. Zhang, Q. Zhang and G. Chen, Carbon Energy, 2020, 2, 408 Search PubMed.
  16. D. Qu, X. Li, H. Wang and G. Chen, Adv. Sci., 2019, 6, 1900584 Search PubMed.
  17. L. Deng and G. Chen, Nano Energy, 2021, 80, 105448 Search PubMed.
  18. J. Chen and L. Li, JETP Lett., 2020, 112, 117 Search PubMed.
  19. X. Mu, X. Wu, T. Zhang, D. B. Go and T. Luo, Sci. Rep., 2014, 4, 3909 Search PubMed.
  20. W. Wang, Q. Zhang, J. Li, X. Liu, L. Wang, J. Zhu, W. Luo and W. Jiang, RSC Adv., 2015, 5, 8988 Search PubMed.
  21. D. Narducci, E. Selezneva, G. Cerofolini, S. Frabboni and G. Ottaviani, J. Solid State Chem., 2012, 193, 19 Search PubMed.
  22. J. Gao, C. Liu, L. Miao, X. Wang, Y. Peng and Y. Chen, RSC Adv., 2016, 6, 31580 Search PubMed.
  23. O. Okhay, G. Gonçalves, C. Dias, J. Ventura, E. M. F. Vieira, L. M. V. Gonçlves and A. Tkachb, J. Alloys Compd., 2019, 781, 196 Search PubMed.
  24. H. Im and J. Kim, Carbon, 2012, 50, 5429 Search PubMed.
  25. J. Choi, N. D. K. Tu, S. S. Lee, H. Lee, H. Kim and J. Kim, Macromol. Res., 2014, 22, 1104–1108 Search PubMed.
  26. K. Wakata, M. R. Karim, M. S. Islam, R. Ohtani, M. Nakamura, M. Koinuma and S. Hayami, Chem. – Asian J., 2017, 12, 194 Search PubMed.
  27. N. T. Hung, A. R. T. Nugraha and R. Saito, Energies, 2019, 12, 4561 Search PubMed.
  28. T. Mehmood, J. H. Kim, D.-J. Lee, S. Dizhur, R. Odessey, E. S. Hirst, R. M. Osgood III, M. H. Sayyad, M. A. Munawar and J. Xu, Mater. Res. Express, 2019, 6, 075614 Search PubMed.
  29. J. Gao, C. Liu, L. Miao, X. Wang, Y. Peng and Y. Chen, RSC Adv., 2016, 6, 31580 Search PubMed.
  30. W. Wang, Q. Zhang, J. Li, X. Liu, L. Wang, J. Zhu, W. Luo and W. Jiang, RSC Adv., 2015, 5, 8988 Search PubMed.
  31. O. Okhaya, G. Gonçalves, C. Dias, J. Ventura, E. M. F. Vieira, L. M. V. Gonçalves and A. Tkach, J. Alloys Compd., 2019, 781, 196 Search PubMed.

Footnote

Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ma00299f

This journal is © The Royal Society of Chemistry 2021
Click here to see how this site uses Cookies. View our privacy policy here.