David E.
Oliver
ab,
Andrew J.
Bissell
b,
Xiaojiao
Liu
a,
Chiu C.
Tang
c and
Colin R.
Pulham
*a
aEaStCHEM School of Chemistry, The University of Edinburgh, Joseph Black Building, David Brewster Road, Edinburgh, EH9 3FJ, Scotland, UK. E-mail: C.R.Pulham@ed.ac.uk
bSunamp Ltd., Macmerry Business Park, 1 Satellite Park, Tranent, EH33 1RY, Scotland, UK
cDiamond Light Source, Diamond House, Harwell Science and Innovation Campus, Fermi Ave, Didcot OX11 0DE, UK
First published on 8th December 2020
This study has identified two polymer additives that when added in low concentrations can be used to reliably prevent incongruent melting of sodium acetate trihydrate (SAT) when temperature-cycled over multiple thousands of melting and freezing cycles. The polymers appear to act as crystal-habit modifiers that at sub-optimal concentrations dramatically alter the morphology of any anhydrous sodium acetate that may be formed, and at higher concentrations completely suppress precipitation of anhydrous sodium acetate. In situ X-ray powder diffraction experiments show that the active nucleator for SAT is Na2HPO4·2H2O, and that the mechanism of thermally induced deactivation is dehydration in solution to form anhydrous Na2HPO4. Based on these studies, new formulations of SAT have been developed that demonstrate consistent and reliable performance as phase-change materials for heat-storage applications.
![]() | ||
Fig. 1 Phase diagram for sodium acetate and water, modified from ref. 5. |
This reflects the fact that at 58 °C the solubility limit of sodium acetate in water is 58.0 wt% (138.10 g/100 ml), whereas sodium acetate trihydrate corresponds to a composition of 60.28 wt% sodium acetate (151.76 g/100 ml), i.e. a significantly higher concentration than the solubility limit of sodium acetate at 58 °C. One potentially simple solution to this problem is to add extra water in order to form a 58 wt% composition that is fully liquid at 58 °C. This should produce a thermodynamically stable solution at 58 °C, i.e. it is neither in the metastable zone nor in the supersaturated zone and thus no solid should precipitate. Nevertheless, it has been observed that temperature cycling of 58 wt% composition did still precipitate anhydrous sodium acetate and even when a 56 wt% composition was cycled 100 times, extensive precipitation of the anhydrous salt was observed.7 Moreover, dilution from the ideal trihydrate composition substantially lowers the freezing temperature and reduces the energy density of the PCM.7 Previous attempts to overcome the incongruent melting of SAT have exploited the use of thickening agents to prevent the precipitation and settling of anhydrous sodium acetate. For example, Cabeza et al. explored the use of starch, bentonite, methylhydroxyethyl-cellulose and methyl-cellulose.8 Of these, the most promising was methylhydroxyethyl-cellulose at a loading of 30 wt%, but this decomposed if heated to above 65 °C. Such high loadings also resulted in a reduction in the latent heat of fusion by up to 35%.8 Wada et al. studied polyvinyl alcohol as a thickener, combined with paraffin oil (1%), acetone (0.5%) and extra water (3.5%).9 They found that the stability of the sample was greatly improved compared to pure SAT. However, variability in the measured value of the latent heat of fusion was still observed, although this aspect was not elaborated on further. More recently Kong et al. have described the use of mixtures of SAT containing carboxy-methyl cellulose, xanthan gum, and unspecified polymers to prevent sub-cooled SAT from precipitating on standing at ambient temperature for extended periods of time.10 These formulations indicated that the energy storage density was retained when compared to samples of pure SAT suffering from phase separation. However, the formulations were not subjected to thermal cycling. Liu et al. have reported a formulation based on SAT adsorbed in micro-porous, expanded vermiculite.11 Thermo-gravimetric results showed that the phase separation problems were almost overcome, and thermal cycling showed that the composite PCM was stable over 150 melting–solidification cycles. The performance improvement of SAT was attributed to the micro-scale phase change and heat transfer within the pores of the expanded vermiculite.11
The second disadvantage of SAT is its strong tendency to sub-cool (super-cool) well below its normal freezing point. Sub-cooling is a consequence of the failure to nucleate crystallisation of the liquid and is a common phenomenon displayed by many salt hydrates. Whilst sub-cooling can be exploited in devices such as disc-activated hand-warming packs, this is a major disadvantage for other applications which require reliable and reproducible freezing of the PCM. Mechanically induced nucleation can be achieved for hand-warming packs through the use of a small metal disc that, when flexed, releases into the liquid tiny seed crystallites that induce nucleation and subsequent crystallisation.12 Seed crystallites are trapped within sub-micron cracks on the surface of the disc and persist even at regeneration temperatures of 100 °C. Nucleation of SAT may also be induced by the addition of additives that include: silicon carbide and bentonite,13 expanded graphite,14 copper nano-particles,15 and chitin nano-whiskers.16 Perhaps the most well-studied and reliable nucleators that have been reported are based on disodium hydrogenphosphate (Na2HPO4, Na2HPO4·7H2O, Na2HPO4·12H2O)8,17,18 and tetrasodium pyrophosphate (Na4P2O7 and Na4P2O7·10H2O).19 However, there are widespread reports about the ‘deactivation’ of these nucleators, i.e. under certain conditions they no longer nucleate SAT when cooled below its melting point.20–24 In particular, when the temperature of samples of SAT containing these nucleators exceeds 80 °C, then nucleation on subsequent cooling becomes sporadic, and when samples are heated above 90 °C, then deactivation of the nucleator is complete and subsequent nucleation fails completely. One explanation that has been presented for this deactivation of the nucleator is that seed crystals of SAT are adsorbed on the surface of the nucleator and persist some way above the melting point of SAT, but at higher temperatures these seed crystals desorb from the surface and then immediately melt.22 However, no experimental evidence has been provided to corroborate this hypothesis.
The twin challenges of incongruent melting of SAT and deactivation of the nucleator continue to severely restrict the use of SAT in heat-storage systems where reproducible performance over multiple thousands of heating/cooling cycles and long-term stability is crucial. The purpose of this study was therefore to identify a reliable method to prevent the incongruent melting of SAT and to investigate the mechanism of deactivation of hydrogenphosphate-based nucleators.
There were several key requirements for the selection of polymers that might prevent incongruent melting of SAT. The primary consideration was solubility, especially as hydrocarbon-based polymers are often only poorly soluble in aqueous solutions on account of their hydrophobic backbone. In recognition that the measured pH of molten SAT is ∼10 and that there is a very high concentration of sodium ions, studies focused on poly-carboxylates, poly-carboxylic acids, poly-amines, poly-alcohols, and poly-ethers. For commercial applications, additional requirements include the following: readily available, non-hazardous, low-cost, and sufficiently low viscosity to enable easy pouring. Initial screening studies investigated the effects on incongruent melting for 55–58 wt% aqueous solutions of sodium acetate with polymers added over the range 1–5 wt%. Samples were repeatedly thermally cycled between 20–60 °C, with crystallisation of the sub-cooled solution initiated by the addition of a crystallite of SAT. The appearance of anhydrous sodium acetate in the melt was monitored visually, and if precipitation occurred then the sample was heated to 75 °C with stirring to re-dissolve the solid. An additional test investigated whether any anhydrous sodium acetate precipitated from a sub-cooled solution on standing for 24 hours at 20 °C. From these studies, two polymer systems showed promising performance: a 1:
2 copolymer of methacrylic acid and methyl methacrylate (Mw in range 500
000–1
000
000), shown in Fig. 2; a 30 wt% aqueous solution of the sodium salt of poly(methacrylic acid) Mw ∼ 9500 by GPC, 30 wt% in H2O, or alternatively, poly(methacrylic acid, sodium salt) solution average Mw 4000–6000, 40 wt% in H2O-see Fig. 2.
![]() | ||
Fig. 2 Structures of (a) poly(methacrylic acid-co-methyl methacrylate) (PMMA-co-MAA – ratio n![]() ![]() ![]() ![]() |
At loadings of 1 wt% these polymers were readily soluble in molten SAT and consistently prevented precipitation of anhydrous sodium acetate from a 58 wt% aqueous solution from both the hot and sub-cooled melts over multiple (>40) heating and cooling cycles. In order to optimise these formulations, experiments were then conducted to establish the upper concentration limit of the sodium acetate solution with a 1 wt% loading of polymer that would not melt incongruently. The limit was found to be 58.24 wt% sodium acetate to 41.76 wt% water, which is in close agreement with the limiting ratio derived from the previously reported phase diagram shown in Fig. 1.5 This corresponds to a slightly water-rich composition NaCH3CO2·(H2O)3.35 compared to SAT. Similar optimisation experiments were conducted to obtain lower limits for the concentrations of polymers required to prevent incongruent melting. These results are summarised in Tables 1 and 2.
Final composition | Weight percentage |
---|---|
Weight ratio of sodium acetate to water = 0.5824![]() ![]() |
|
PMMA-co-MAA | 0.80% |
Sodium acetate | 57.78% |
Water | 41.42% |
Final composition | Weight percentage |
---|---|
Weight ratio of sodium acetate to water = 0.5824![]() ![]() |
|
Na-PMAA | 0.67% |
Sodium acetate | 57.85% |
Water | 41.48% |
Differential scanning calorimetry (DSC) measurements (at heating rates of 10 °C min−1) were conducted to ascertain the effect of the polymer additives and additional water on both the melting points and the latent heat of these formulations. Consistent melting points of 58 °C and enthalpies of fusion of 218 kJ kg−1 (278 kJ dm−3) were obtained (see ESI†), thereby demonstrating that these compositions retain acceptably high energy densities.
When experiments were conducted using a sub-optimal amount (0.5 wt%) of the Na-PMAA polymer and on standing for a period of two weeks in a sub-cooled state at 20 °C, precipitation of a mass of extremely thin needles was observed (Fig. 3a). Despite the effects of strong preferred orientation, the powder X-ray diffraction pattern identified this material as anhydrous sodium acetate.26 However, the observed crystal morphology was very different from the much larger, plate-shaped crystals of anhydrous sodium acetate that crystallise from an aqueous solution in the absence of the polymer (see Fig. 3b). This indicates that the polymer is acting as a crystal-habit modifier that dramatically changes the morphology of anhydrous sodium acetate crystallites. Moreover, it was observed that these needle-shaped crystals rapidly dissolved on heating the solution to 60 °C, and much more readily than the plate-like crystals formed in the absence of the polymer. This presumably reflects the much larger surface area-to-volume ratio of the needles. Hence it appears that at high concentrations the polymer inhibits formation of anhydrous sodium acetate, and at lower concentrations it modifies the morphology of any anhydrous sodium acetate formed such that it readily dissolves on heating.
Both polymers displayed a striking ability to inhibit nucleation of anhydrous sodium acetate. However, it is clear from these experiments that chain length, molecular weight, and viscosity are not dominant factors the suppression mechanism, i.e. PMMA-co-MAA has a much longer chain length and molecular weight than Na-PMAA, and results in a much more viscous solution than Na-PMAA. Moreover, other highly viscous samples failed to prevent incongruent melting e.g. poly(acrylamide) with Mw = 5–6000
000.
At present, the mechanism of action of the two polymers is not known. We can speculate that at a pH of 10, both polymers contain carboxylate groups that could bind strongly with sodium ions associated either with pre-nucleation clusters or with particular surfaces of small crystallites. The hydrophobic alkyl chains would then prevent further attachment of other ions to these clusters or to particular crystal faces. However, this remains conjecture at this stage.
In order to gain further insight into the thermally induced mechanism for the deactivation of Na2HPO4, we conducted in situ, variable temperature powder X-ray diffraction experiments using Beamline I11 at the Diamond Light Source, UK.27,28 This high-intensity synchrotron source, combined with this beamline's high-resolution capability and sensitive detectors, allowed complete diffraction patterns from weakly scattering samples in thin-walled capillaries to be recorded with a scan time of 2 seconds. Samples were prepared by dissolving anhydrous sodium acetate in deionised water in a glass vial with addition of PMMA-co-MAA and a small quantity of anhydrous Na2HPO4 (see Experimental details for full procedure‡).
Fig. 4(a)–(e) show the sequence of X-ray powder diffraction patterns of SAT and nucleator recorded under different conditions. Fig. 4(a) shows the pattern obtained for the initial loading of the capillary at 25 °C, and two polycrystalline components can readily be identified by comparison with reference patterns: namely SAT and Na2HPO4. Fig. 5 shows the experimental pattern for the initial loading fitted with a Rietveld refinement to SAT and Na2HPO4·2H2O, using as starting points the crystal structures of SAT (CSD identifier code NAACET01)29 and Na2HPO4·2H2O (ICSD collection code 1289).30 All of the Bragg peaks in the experimental pattern can be fitted to a mixture of SAT and Na2HPO4·2H2O, and no signs of anhydrous Na2HPO4 or any of the other known hydrates [Na2HPO4·7H2O, Na2HPO4·12H2O] were detected.
Fig. 4(b) shows the pattern obtained on initially warming to 62 °C. All of the SAT melted and this contributes to the amorphous background observed in the pattern. The remaining Bragg peaks originate entirely from the Na2HPO4·2H2O that remained suspended in the liquid. On cooling the sample, crystallisation of SAT occurred with no appreciable sub-cooling. Fig. 4(c) shows the pattern recorded at 25 °C and although inevitably there is a high degree of preferred orientation caused by crystallisation of SAT within the capillary, all of the peaks can be assigned to a mixture of SAT and Na2HPO4·2H2O.
Fig. 4(d) shows the pattern recorded when the sample was subsequently warmed to 90 °C. Again, all of the SAT melted, but on this occasion, peaks from Na2HPO4·2H2O disappeared and were replaced with a new set of peaks that can be assigned to anhydrous Na2HPO4, by comparison with the reference pattern simulated from the crystal structure of Na2HPO4 (ICSD collection code 81304).31Fig. 6 shows this in more detail – Rietveld refinement of the pattern recorded at 90 °C shows that anhydrous Na2HPO4 is the only polycrystalline phase present. On cooling to 25 °C, Fig. 4(e) shows that SAT failed to crystallise and that anhydrous Na2HPO4 persisted. Hence it appears that heating to 90 °C results in thermally induced dehydration of the dihydrate to form the anhydrous form, which persists on cooling to 25 °C (see ESI† for corresponding Rietveld refinement), and that the anhydrous form fails to prevent sub-cooling of SAT.
This set of in situ experiments therefore shows that the active nucleator for SAT is actually the dihydrate, Na2HPO4·2H2O, and that the mechanism of thermally induced deactivation is dehydration in solution to form anhydrous Na2HPO4. Hence, this provides an explanation for the observation in bulk samples that deactivation of the nucleator was dependent not only on temperature, but also on the time held at elevated temperature and the quantity of nucleator added. Further support for this dehydration mechanism is provided by the results of a combined TGA/Raman study that mapped the sequential thermally induced dehydration of Na2HPO4·12H2O in the solid phase.32 Five dehydration events were observed and the following compounds were sequentially identified: Na2HPO4·8H2O, Na2HPO4·7H2O, Na2HPO4·2H2O, Na2HPO4·H2O, and Na2HPO4. Under the conditions of a flowing nitrogen stream, Na2HPO4·2H2O began to dehydrate to the monohydrate at 72 °C, with further dehydration to the anhydrous salt at 82 °C.32 One remaining question is why the addition of anhydrous Na2HPO4 to bulk samples of SAT appears to promote reliable nucleation. This is because the sparingly soluble Na2HPO4 recrystallises from solution as the dihydrate under certain conditions, and especially when SAT freezes, thereby explaining why nucleating behaviour can be regenerated either by reducing the temperature of sub-cooled samples to below 0 °C or adding a seed crystal of SAT in order to promote crystallisation of the entire sample. Based on these results, it seems likely that a similar thermally induced dehydration mechanism is responsible for the deactivation of Na4P2O7 when used as nucleator. Only the decahydrate and the anhydrous form are known and so dehydration of the decahydrate may be responsible for its deactivation. This is supported by the observation that the melting point of Na4P2O7·10H2O is reported to be in the range 69–79 °C.33 The in situ temperature-cycling experiments also showed that no anhydrous sodium acetate was ever observed for any of the compositions containing either of the polymer additives, thereby confirming that incongruent melting was successfully prevented. The results of these studies allowed us to develop an optimum formulation based on Na-PMAA with the composition shown in Table 3.
Final composition | Weight percentage |
---|---|
Na-PMAA polymer | 0.67% |
Sodium acetate | 56.67% |
Water | 40.63% |
Na2HPO4·2H2O | 2.02% |
Extended lifetime testing in a Sunamp heat battery shows that this PCM formulation performs reproducibly over >40000 cycles. Independent testing of this PCM formulation has also been conducted by the RAL Quality Association PCM and the results show no deterioration of performance over >10
000 heating and cooling cycles according to the testing regime described in RAL-GZ 896.34
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0ce01454k |
‡ Experimental details for the in situ X-ray powder diffraction studies: 8.1896 g of anhydrous sodium acetate was added to 5.9427 g of deionised water, together with 0.1213 g poly(methacrylic acid-co-methyl methacrylate) and 0.2824 g of anhydrous Na2HPO4 in a glass vial. The sample was heated to 70 °C with occasional shaking to dissolve any remaining SAT. The sample was then cycled repeatedly (>8 times) between 20 °C and 65 °C, and maintained at the highest temperature in order to ensure complete dissolution of any seed crystals of SAT. Congruent melting was observed on heating and spontaneous crystallisation was observed on cooling to 58 °C. Initial attempts to load a 0.7 mm diameter borosilicate capillary directly from the liquid melt (using capillary action) were unsuccessful – no crystallites of Na2HPO4 could be detected in the capillary. Instead the sample was heated to 65 °C, vigorously shaken and then allowed to settle for 10 seconds. Half of the liquid sample was then decanted off and the remainder was then shaken. A small aliquot was poured into a chilled mortar, where crystallisation occurred immediately. The sample was ground to a fine powder with a pestle and mortar, and then loaded into a 0.7 mm capillary. The open end of the capillary was then sealed with superglue adhesive and mounted on the diffractometer operating with a wavelength of 0.82694 Å. The capillary was rotated at 360 rpm in order to achieve acceptable powder averaging, and the temperature was controlled using an Oxford Cryosystems Cryostream. Using the PSD Mythen detector, it was possible to collect high-quality patterns with scan times of 2 s. |
This journal is © The Royal Society of Chemistry 2021 |