Open Access Article
Xiang
Luo‡
ab,
Xianbo
Lu‡
c,
Ya
Chen‡
d,
Xiaodong
Chen
*abe,
Hele
Guo
a,
Chunyu
Song
a,
Nannan
Wang
*a,
Dawei
Su
b,
Guoxiu
Wang
b,
Lifeng
Cui
*a and
Yan
Liu
*a
aSchool of Materials Science and Engineering, Dongguan University of Technology, Dongguan 523808, Guangdong, China. E-mail: chenxd@dgut.edu.cn; wangnn@dgut.edu.cn; lcui@dgut.edu.cn; liuyan26914@163.com
bCenter for Clean Energy Technology, School of Mathematical and Physical Science, Faculty of Science, University of Technology Sydney, NSW 2007, Australia
cR&D Center, Shanghai Kingfa Sci. & Tech. Co., Ltd, Shanghai 201714, China
dSchool of Physical Science and Technology, ShanghaiTech University, Shanghai 201210, China
eDepartment of Applied Chemistry, School of Science, Xi'an Jiaotong University, Xi'an 710049, Shaanxi, China
First published on 7th October 2020
The development of commercial lithium–sulfur (Li–S) batteries is typically restricted by the intrinsic drawbacks of the dissolutiion and shuttling of lithium polysulfides (LPS) and the uncontrollable growth of lithium dendrites. To address these non-ignorable challenges, a multifunctional composite nanofiber-based separator consisting of an electrospinning polyimide (PI) substrate and a polyamide–polyvinyl alcohol (PA–PVA) top layer is designed and fabricated via interfacial polymerization (IP). In this situation, its superior features, such as desirable wettability, suitable porosity, excellent electrolyte uptake and retention, and high thermal tolerance, can be obtained. Besides, the architecture of the highly negatively charged PA–PVA top layer with a dense Turing structure can not only provide an electronegative environment to accelerate the Li+ transmembrane transfer as well as simultaneously repel the negatively charged polysulfide ions, but also enable ordered Li+ migration for homogeneous Li deposition on the anode. Due to these advanced structural characteristics, the Li–S battery assembled with the PI/PA–PVA separator gives a high initial specific capacity of 1499 mA h g−1 at 0.1C and a stable discharge capacity of 852 mA h g−1 with an ultralow fading rate of 0.1% per cycle after 500 cycles at 0.2C. More importantly, this PI/PA–PVA top layer has the functional characteristics of melting and self-closing at high temperatures, endowing the Li–S battery with excellent safety performance.
Up to now, to resolve the challenge of LPS shuttling, multiple strategies, including the use of an ionic liquid electrolyte11 and a modified structure sulfur host,12 have been adopted. Besides, persistent efforts have also been made to dismiss the growth of Li dendrites by protecting the lithium anode, including the fabrication of protective layers on anodes,13–16 the development of all-solid-state electrolytes,17–20 the addition of functional species in solid electrolyte interphase (SEI),21 and the use of three-dimensional scaffolds.22 Nevertheless, as a matter of fact, these methods typically only settle the problems of the cathode or anode solely. Therefore, it still remains a great challenge to suppress the growth of Li dendrites and the shuttle effect simultaneously. Notably, to address these two concerned issues for Li–S batteries, the fabrication of a novel separator has attracted widespread attention as it occupies the most important component in the Li–S battery, which can serve as an insulator to avoid the internal short circuit between the cathode and anode, as well as penetrate adequate electrolyte to ensure efficient Li+ transport.23–27 More importantly, it has been demonstrated that the shuttle effect of LPS and the growth of lithium dendrites can be concurrently suppressed to some extent by tailoring the structures and properties of separators, such as coating the separator with carbon materials,25,28,29 metal organic frameworks,30–33 metal oxides,34–36 negatively charged polymers,37–40 and so on. Although some positive effects have been observed as expected, there still remain defects that affect the battery cycle life seriously. In particular, the distributed pores over the separator could be inevitably blocked by the modified coating layer, which results in poor Li+ migration throughout the separator, thus contributing no capacity and even reducing the energy density of the Li–S battery.41–44
In response to this situation, it is essential for the separator to enhance the permeability of Li+ migration when being coated with a modified layer. In 1981, John Cadotte et al. firstly reported that interfacial polymerization is a facile and effective method to prepare composite membranes with negatively charged polyamide (PA) thin films containing nano-sized pores on porous supports.45 Recently, Gao and co-workers further concluded that PA nanofilms with Turing structures presents a significantly improved specific surface area and more permeation sites, thus contributing to better permeability compared to the smooth ones.46 On the other hand, the porous substrate can also influence the sieving and permeating performance of composite membranes, for which electrospinning nanofiber membranes are promising candidates as compared with traditional phase-inversion substrates due to their high porosity, large pore size and good connection of the pores.47,48 With the aforementioned advantages, we design a novel polyimide/polyamide–polyvinyl alcohol (PI/PA–PVA) composite separator consisting of a functional PA–PVA top layer with a Turing structure and a PI nanofiber substrate (Fig. 1a). The PI nanofiber substrate provides not only excellent electrolyte uptake but also good thermal stability. Moreover, the more negatively charged PA–PVA top layer with nanopores can suppress the shuttling of LPS attributed to the electrostatic repulsion, hence preventing the deterioration of electrochemical performance. Above all, the existing synergetic effects between them will greatly accelerate the transfer of Li+ through the separator as well as promote the homogeneous deposition of lithium on the anode, which are conducive to strengthening the stability of the SEI layer and inhibiting the growth of Li dendrites (Fig. 1b). When a Li–S battery with the PI/PA–PVA separator is confronted with high temperatures, the appropriate melting point of the PA–PVA top layer can make it available to melt and self-close to block the separator pores while the thermally stable PI framework can preserve the whole dimension of the separator. As a consequence, the Li–S battery with the PI/PA–PVA separator gives a high initial specific capacity and a stable discharge capacity. This facile fabrication strategy provides a cost-effective pathway for the large-scale production of high-performance separators and the practical application of high-energy-density Li–S batteries.
Furthermore, the wettability, porosity and electrolyte uptake and retention of these separators were also quantitatively examined because these inherent properties take the prominent function in the comprehensive performance of Li–S batteries. The wettability of the separators for the electrolyte was typically evaluated via contact angle measurements. As shown in Fig. 2a and Table S1 (ESI†), it can be observed that the contact angle of the PI/PA–PVA separator is measured to be 0°, which is equal to that of the PI separator (0°) but significantly lower than that of the PI/PA separator (35.8°), indicating its favourable affinity toward the electrolyte. As for the Celgard separator, its contact angle raises to 49.2°, hence resulting in an unsatisfactory adsorption ability for the electrolyte.54,55 Then the membrane porosity of separators was analyzed using a liquid absorption method as it is mainly responsible for the electrolyte uptake performance in a battery system.26 Benefiting from the interconnected fibrous structure of nanofiber membranes, even though the porosity of the PI/PA–PVA separator was determined to be 75.1% smaller than those of the PI/PA (76.6%) and PI separators (92.1%) as shown in Table S1 (ESI†), it is still much higher than that of the Celgard separator (41.3%), thus approving the electrolyte uptake. Accordingly, the electrolyte uptake values of PI, PI/PA and PI/PA–PVA separators were calculated to be 2011%, 1321% and 1640%, respectively, while it declines to 156% for the Celgard separator under steady state conditions after 15 minutes, as demonstrated in Fig. 2b and Table S1 (ESI†). In addition, the electrolyte retention capability is another crucial parameter to determine the durability of the liquid electrolyte entrapped in the separators. As displayed in Fig. 2c and Table S2 (ESI†), when stored at 50 °C, the electrolyte retention values of PI and PI/PA–PVA separators were stabilized at 70.2% and 52.6% after 80 min, whereas it decreases to 41.1% for the PI/PA separator after 80 min, and merely 11.5% for the Celgard separator after 190 min. Through the above comparison, it is known that the PI/PA–PVA separator affords the best electrolyte retention capability among these separators. Therefore, the introduction of the electronegative PA–PVA top layer with a dense Turing structure can not only improve the polarity of the PI/PA–PVA separator to provide better affinity toward the electrolyte but also availably block the electrolyte inside this separator.
The thermal stability of the separator can be assessed by gauging its dimensional change under different gradient temperature conditions, which is related to the Li–S battery safety. As shown in Fig. 2d, the commercial Celgard separator shrinks and curls quickly and is eventually destroyed as the heating temperature increases from 100 °C to 150 °C.56,57 On the contrary, no visible dimensional variation occurs for PI and PI/PA–PVA separators in this temperature range, which is due to the excellent thermo-tolerance of the PI substrate. Furthermore, DSC measurements illustrate that there are two endothermic peaks at 136.5 °C and 166.2 °C in the curve of the Celgard separator while no apparent peaks can be recognized for the PI separator (Fig. 2e). Regarding the PI/PA–PVA separator, there are two endothermic peaks appearing at around 100 °C and 230 °C in the DSC curve, which are indexed to the melting point of PA and PVA ingredients, respectively. Besides, the TGA indicates that the weight loss of the Celgard and PI separators starts from about 295 °C and 414 °C, respectively (corresponding to 10wt% loss, Fig. 2f), whereas, for the PI/PA–PVA separator, the weight loss can be divided into three stages at about 308 °C, 350 °C and 532 °C, which are ascribed to the thermal degradation of PVA, PA and PI components, respectively. These results elucidate that the PA–PVA top layer will melt itself and block the separator pores at high Li–S battery working temperatures, while the PI substrate can maintain the complete dimension of the separator due to its excellent thermal tolerance. Consequently, its unique self-closing property can protect the batteries from short circuit at high working temperatures, which is significantly beneficial for the Li–S battery safety (Fig. S4b, ESI†).
The retarding ability of the separators for LPS can be considered as an indispensable parameter for the Li–S battery performance, which can be visually judged by diffusion tests that are conducted with a double-L device when the Li2S6 solution and pristine electrolyte are separated by two different membranes. As shown in Fig. S5a (ESI†), the palpable transmembrane penetration of LPS can be clearly detected for this device with the Celgard separator, while the electrolyte still remains clear even after 12 h when the PI/PA–PVA separator is utilized in this system, demonstrating its effectively prohibitive diffusion for LPS in the electrolyte solution (Fig. S5b, ESI†). This is mainly attributed to the highly negatively-charged environment constructed by the introduction of the PA–PVA top layer onto the PI substrate (Fig. S1, ESI†), which can restrain the electronegative LPS via electrostatic repulsion. At the same time, the Li–S battery performance is also crucially dependent on the Li+ transport property throughout the separators. Hence, the Li+ transference number and ionic conductivity were determined via AC impedance and chronoamperometry and EIS analysis as shown in Fig. 3a–d and Fig. S6 (ESI†), and the relevant results are shown in Fig. 3e. It can be seen that the Li+ transference numbers of PI, PI/PA, PI/PA–PVA and Celgard separators were calculated to be 0.54, 0.50, 0.70 and 0.45, respectively. Accordingly, the PI/PA–PVA separator shows the highest Li+ transference number among these separators. Moreover, the PI/PA–PVA separator reveals an excellent ionic conductivity of 2.28 when compared with PI (1.0), PI/PA (0.81), and Celgard separators (0.61). From the above results, although the membrane porosity of the PI/PA–PVA separator decreases after interfacial polymerization, the corresponding Li+ transference number and ionic conductivity still increase. This certainly benefits from its better electrolyte affinity and the highly electronegative PA–PVA top layer, which would facilitate the positively charged Li+ transport via electrostatic attraction. In contrast, the Celgard separator shows unsatisfied Li+ transfer ability and ionic conductivity due to its poor electrolyte affinity, low porosity and inferior electrolyte uptake and retention. Besides, from the I–V curves of the Li–S batteries assembled with PI, PI/PA–PVA and Celgard separators as shown in Fig. 3f, it can be concluded that the use of the PI/PA–PVA separator in Li–S batteries occupies a much broader electrochemical stability window than the other two separators, demonstrating that its appealing application can be extended to the field of high voltage Li–S batteries. Moreover, the open circuit voltage (OCV) was applied here to illustrate the self-discharge behaviour of Li–S batteries with PI, PI/PA, PI/PA–PVA and Celgard separators. As shown in Fig. S7 (ESI†), the OCVs of Li–S batteries with PI, PI/PA and Celgard separators decay seriously to 2.45 V, 2.55 V and 2.50 V in just a few hours, respectively. However, the OCV still maintains a larger value of 2.64 V after 13 h for the PI/PA–PVA separator. These results confirm that the self-discharge phenomenon can be effectively depressed in Li–S batteries when utilizing the PI/PA–PVA separator.
The CV curves of the Li–S batteries assembled with PI/PA–PVA, PI and Celgard separators at a scan rate of 0.1 mV s−1 are displayed in Fig. 4a and Fig. S8a, b (ESI†). Obviously, there are two cathodic peaks appearing at around 2.35 V and 2.10 V corresponding to the reduction of sulfur to long-chain LPS (SX2−, 4 < X ≤ 8) and further reduction to Li2S2 or Li2S, respectively. Meanwhile, the anodic peaks at around 2.33 V and 2.42 V are relative to the oxidation of LPS to sulfur.58 Compared with Li–S batteries with PI and Celgard separators, the CV curves of the initial three cycles are nearly overlapped for the Li–S battery with the PI/PA–PVA separator, indicating its high reversibility and improved LPS redox kinetics. In addition, to investigate the Li+ diffusion coefficients (DLi+) for these separators, the CV curves obtained at different scan rates were recorded (Fig. 4b and Fig. S8c, d, ESI†).59 The values can be calculated from the slope of the linear fitting curve between the square root of scan rate (V0.5) and the peak current (Ip) using Randles–Sevcik equation (Fig. 4c and Fig. S8e, f, ESI†), and the results are summarized in Fig. S9 (ESI†). The Li–S battery fabricated with the PI/PA–PVA separator possesses the highest Li+ diffusion coefficients (DLi+ (O2) = 5.13 × 10−6, DLi+ (R1) = 3.97 × 10−6, DLi+ (R2) = 2.09 × 10−6) among these separators even though its PI nanofiber substrate is covered by a dense top layer. These results demonstrate that the successful architecture of the negatively charged PA–PVA top layer imparts the PI/PA–PVA composite separators with strong inhibitive ability for LPS and a high Li+ diffusion coefficient when integrated with a Li–S battery.
The electrochemical kinetics of Li–S batteries assembled with PI, PI/PA, PI/PA–PVA and Celgard separators were determined using the EIS analysis as shown in Fig. 4d. The charge-transfer resistance (Rct) of Li–S batteries with PI nanofiber-based separators is rather smaller than that of the Celgard separator (91 Ω). Among them, the Rct of the Li–S battery with the PI/PA separator is much increased as compared with the value of the battery with the PI separator since the distributed pores over the PI nanofiber membrane are fully covered by the PA top layer. However, by comparison, the Rct can be further decreased for the Li–S battery with the PI/PA–PVA separator due to its formation of the PA–PVA top layer with a Turing structure with approvable features such as a high specific surface area, abundant permeation sites and desirable electrolyte affinity, which are beneficial for its faster Li+ diffusion rate. The relationships between the linear fittings of Z′ and the square root in the low-frequency region (ω−0.5) are shown in Fig. 4e, the slope of which represents the Warburg factor to determine the Li+ diffusion transportation.60 It can be observed that the slopes of Li–S batteries with PI, PI/PA and PI/PA–PVA separators are 12.2, 63.1 and 43.4, respectively, which are much less than that for the Celgard separator (80.1), further confirming that the PI nanofiber-based separators show better Li+ transportation in the Li–S battery. The galvanostatic discharge–charge profiles of Li–S batteries assembled with PI, PI/PA–PVA and Celgard separators at 0.1C are displayed in Fig. 4f. The two plateaus on discharge curves represent the redox of sulfur to long-chain LPS and further to short-chain LPS, while the plateau on charge curves refer to the transition of short-chain LPS to sulfur. Apparently, the Li–S battery with the PI/PA–PVA separator exhibits a much lower overpotential than those with the PI and Celgard separators, indicating its superior electrochemical reversibility.
In order to further unveil electrochemical properties, the discharge–charge curves at different C-rates are analyzed for Li–S batteries with these separators (Fig. 5a–c and Fig. S10, ESI†). It can be seen that all of the discharge curves display a typical two-plateau characteristic under lower current densities. In this regard, the PI/PA–PVA separator affords the highest specific capacity among them, which decreases with increasing the current rate from 0.1C to 5C. In particular, the initial specific capacity of the Li–S battery with the PI/PA–PVA separator can reach values as high as 1499 mA g−1 at 0.1C. Besides, when the current-rate is switched from 5C back to 0.1C, the Li–S battery assembled with the PI/PA–PVA separator has exhibited better recovery ability of discharge capacity than those with PI, PI/PA and Celgard separators, thus reflecting its excellent stability (Fig. 5d). Furthermore, the cycle stabilities of Li–S batteries assembled with these separators were further evaluated at 0.2C. As shown in Fig. 5e, their rapid capacity loss during the initial cycles are mainly triggered by the formation of SEI and the dissolution and shuttling of lithium polysulfides.61–63 More specifically, for the PI separator, the high initial capacity decays very fast in the subsequent cycles, but its decay rate is much lower than that of the Celgard separator. After interfacial polymerization of the PI/PA separator, the cycle stability of the Li–S battery is promoted because of the inhibited shuttling of LPS and the better Li+ transportation by the negatively charged PA top layers.64 Moreover, the electronegativity of the PA layer is further enhanced after the addition of PVA for the formation of the PI/PA–PVA separator, which in turn guarantees a high utilization rate of the S active component and strengthens the cycle stability of the Li–S battery (Fig. 5f). It can be inferred that the loss phenomenon of the S active component on the cathode of the Li–S battery with the PI/PA–PVA separator can be effectively restrained, which can also be visually identified via energy dispersive X-ray spectroscopy (EDS) (Fig. S11, ESI†). As a consequence, the Li–S battery with the PI/PA–PVA separator presents a stable discharge capacity of 852 mA h g−1 with an ultralow fading rate of 0.1% per cycle after 500 cycles (Fig. 5g and Table S2, ESI†).
Furthermore, Li/Li symmetric batteries were integrated with PI/PA–PVA and Celgard separators in order to investigate the interfacial stability of the Li anode in the electrolyte. It can be observed from Fig. 6a that both batteries display relatively high overpotentials in the first few cycles due to the electrode activation and the formation of the SEI layer.65 For the Li–S battery with the PI/PA–PVA separator, the striping and plating of Li gives a low and stable overpotential below 100 mV for over 600 h, indicating a uniform Li deposition and a stable SEI layer formed on the anode. In contrast, the Li–S battery with the Celgard separator exhibits an ultrahigh and unstable overpotential which is more than 200 mV and it increases gradually with cycle time. This unwanted phenomenon mainly results from the formation of Li dendrites on the anode in Li–S batteries, thus causing the continuous destruction and rebuilding of the SEI layer. Besides, the surface morphologies of the Li anode before and after cycling were analyzed via SEM characterization. The pristine Li tablet has a flat and smooth surface morphology (Fig. S12, ESI†). After cycling of the Li–S battery assembled with the Celgard separator, the Li anode was corroded seriously accompanied with visible Li dendrites (Fig. 6b). In contrast, the Li anode remains relatively flat when using the PI/PA–PVA separator (Fig. 6c). In addition, the EDS mapping analysis visually illustrates that there is a large amount of sulfur remaining on the Li anode when using the Celgard separator, which is ascribed to the diffusion of LPS (Fig. 6d). But, for the battery using the PI/PA–PVA separator, there is little sulfur left on the Li anode after cycling (Fig. 6e). The above evidence directly demonstrates that the PI/PA–PVA separator can prevent the Li anode from the shuttle effect of LPS and dendrite growth simultaneously. This is mainly because the negatively charged PA–PVA layer with a dense Turing structure can not only suppress the LPS shuttling through the separator, but also promote the rapid and uniform transmembrane diffusion of Li+ which results in decelerated Li+ depletion and improved homogeneous Li deposition.
000–124
000, 87–89% hydrolyzed), pyromellitic dianhydride (PMDA) and 4,4′-oxydianiline (ODA) were purchased from Sigma-Aldrich. N-Hexane and N,N-methyl-2-pyrrolidone (NMP) were supplied by Shanghai Chemistry Company, which were further dehydrated with CaH2 and purified via further distillation.
The porosity of the separators was characterized through a liquid absorption method and calculated according to the following eqn (1):66
| Porosity = (Ww − Wd)/(ρ × V) | (1) |
The electrolyte uptake and retention of the separators is calculated through the following eqn (2):
| Electrolyte uptake = (W1 − W0)/(W0 × 100%) | (2) |
| Electrolyte retention = [(Wx − W0)/(W1 − W0)] × 100% | (3) |
:
1 by volume) with 2 wt% LiNO3. The galvanostatic discharge–charge performance was tested on a battery-testing system (LAND CT2001A, Wuhan, China). Cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS) were conducted on an electrochemical workstation (CHI660E, Wuhan, China) with the voltage ranging from 1.7 to 2.8 V.
The ionic conductivity was detected via EIS with the frequency ranging from 0.1 Hz to 100 kHz and calculated according to the following eqn (4):
| ó = L/(Rb × A) | (4) |
The lithium ion transference number (tLi+) of the separators was also evaluated via EIS combined with chronoamperometry, which can be calculated according to the following eqn (5):67
| tLi+ = Is(ΔV − I0R0)/I0(ΔV − IsRs) | (5) |
Linear sweep voltammetry (LSV) was performed on another electrochemical workstation (CHI660D, Wuhan, China) with a scan rate of 1 mV s−1. The cells used for this measurement were fabricated by placing the separator between a stainless steel and a lithium foil.
Footnotes |
| † Electronic supplementary information (ESI) available: Photograph of the synthesized PAA in NMP solution; surface zeta potentials of different separators; FTIR spectra of different separators; SEM image of the Celgard separator; SEM images of cross-section of PI/PA–PVA separator; photographs showing the polysulfide diffusion across the Celgard and PI/PA–PVA separators for different time; chronoamperometry profile of the PI/PA separator and the corresponding impedance values; open circuit voltage profiles showing the self-discharge behavior of Li–S batteries with PI, PI/PA–PVA and Celgard separators; CV curves of Li–S batteries with PI and Celgard separators; Lithium ion diffusion coefficients for different separators; discharge–charge profiles of Li–S batteries with the PI/PA separator at different rates; elemental mappings of sulfur on the cathode faced with Celgard and PI/PA–PVA separators after rate test; SEM image of the pristine lithium anode. See DOI: 10.1039/d0ma00653j |
| ‡ These authors contributed equally to this work. |
| This journal is © The Royal Society of Chemistry 2020 |