Open Access Article
Boya
Xiong
ae,
Prakash
Purswani
d,
Taylor
Pawlik
c,
Laxmicharan
Samineni
c,
Zuleima T.
Karpyn
d,
Andrew L.
Zydney
*c and
Manish
Kumar
*bc
aDepartment of Civil and Environmental Engineering, Massachusetts Institute of Technology, USA. E-mail: boyax@mit.edu
bDepartment of Civil and Environmental Engineering, The Pennsylvania State University, USA. E-mail: manish.kumar@psu.edu
cDepartment of Chemical Engineering, The Pennsylvania State University, USA. E-mail: zydney@engr.psu.edu
dJohn and Willie Leone Family Department of Energy and Mineral Engineering, The Pennsylvania State University, USA
eDepartment of Civil, Environmental and Geo- Engineering, University of Minnesota, Minneapolis, MN 55455, USA. E-mail: bxiong@umn.edu
First published on 18th November 2019
Degradation of drag reducer polyacrylamide under high volume hydraulic fracturing (HVHF) conditions alters its polymer size, distribution and chemical composition, potentially affecting the toxicity and treatability of the resulting wastewater. This study focused on a non-chemical pathway-mechanical degradation of polyacrylamide under ultra-high fluid strain conditions (∼107 s−1) that uniquely exist during HVHF but has not yet been explored experimentally. PAM solutions were subjected to an abrupt contraction into a narrow capillary driven by a high-pressure precision pump (∼10
000 psi). The change in polyacrylamide size distribution was evaluated by size exclusion chromatography. The peak polymer molecular weight (MW) after a single-pass through the capillary decreased from 107 to 7 × 105 Da at deformation rate
= 4 × 106 s−1. The extent of degradation increased with
, approximately following an empirical scaling relationship of
for the polyacrylamide with an initial MW ≈ 107 Da. Degraded PAM with lower MW (<106 Da) showed minimal degradation during multiple flow passes even at high deformation rates, suggesting that most mechanical degradation occurs at the first entrance into the fracture. Relative to chemical degradation, mechanical degradation caused a narrowing of the MW distribution due to greater degradation of the larger MW polymers and preferential mid-chain polymer scission. In addition, we saw no detectable change in chemical composition during mechanical scission, in contrast to the generation of carbonyl groups during oxygenic radical induced chemical degradation. Combining both chemical and mechanical mechanisms during HVHF operation, we propose an initial mechanical breakage of polymer chain by fluid strain, followed by chemical degradation under the high temperature and appropriate mineralogical conditions. These findings provide critical information for understanding the nature of degradation byproducts from polyacrylamide, and the treatability of polyacrylamide fragment-containing wastewaters.
Water impactHere we explore a non-chemical mechanism-mechanical degradation of polyacrylamide under ultrahigh shear rates unique to high volume hydraulic fracturing operations. The fundamental understanding enables us to estimate the extent and chemistry of degradation given geological and operational conditions. Such estimation will facilitate fracturing fluid chemists, well operators and regulators to manage chemical usage, characterize and treat fracturing wastewaters, and mitigate risks of environmental releases. |
000 psi (ref. 4)). Long-chain PAM acts as a friction reducer, suppressing turbulent vortices and thereby reducing pumping cost.5,6 Low levels of mechanical chain scission can occur under low strain rates (<105 s−1), similar to those encountered during flow through valves, pipes, and the wellbore, decreasing the polymer MW and lowering the degree of drag reduction.7
Previous studies have demonstrated the loss in viscosity and drag reduction for dilute and semi-dilute PAM solutions due to chain rupture in both laminar and turbulent extensional flow, e.g., upon flow into an abrupt or tapered contraction.8–15 PAM degradation has also been observed in porous media, but this might not be applied in the context of HVHF due to limited transport of hundred-nanometer size polymer coils into the nano- to micro-Darcy range pores in tight shale formations.16,17 Most studies have only focused on evaluating changes in viscosity, with no detailed information presented on the actual changes in polymer molecular size distribution and chemical composition.18 However, the polymer molecular size distribution was found to be determine the fouling potential during wastewater treatment using microfiltration membranes;19 and chemical composition is critical in estimating the persistence, mobility and toxicity of degraded molecules in wastewater.20 Limited estimates of MW changes have been reported using the Mark–Houwink–Sakurada equation but the accuracy of this approach is questionable due to the large variation of the model coefficients with MW distribution, chemical structure, and the presence of solution impurities.21
Capillary flow geometry has previously been utilized to study polymer degradation in reservoir flow,10,22 and can potentially better simulate hydraulically stimulated fracture flow. Such flow with an abrupt contraction entrance contains shear and extensional fluid component,23 both of which contribute to fluid stress but seem to play different roles in polymer scission. In particular, the extensional flow at such geometry is transient instead of quasi-steady state stagnant (as encountered in cross-slot geometry), under which coiled polymer chain only partially extend.24 Jouenne et al.22 compared the extent of PAM degradation (determined from the change in viscosity) in a capillary constriction, porous media, and a blender. Degradation was found to be governed by the extensional flow at the capillary entrance instead of the wall shear inside the capillary tube, as data obtained with capillaries of different length showed the same degree of degradation when plotted in terms of the flow rate (and not the pressure drop). In addition, the extent of degradation increased with increasing time (in the blender) and with increasing number of passes (for flow into the capillary), approaching an asymptote after extended exposure/passes. Vanapalli et al. developed a turbulence theory based scaling correlation that can be applied to a variety of flow geometries including abrupt contraction. Such scaling correlation explains, in addition to extensional flow stress, scission of extended polymer chain is also likely caused by the fluid tension from velocity fluctuation at Kolmogorov scale of turbulence.25 However, these experiments were limited to very low shear rates (<105 s−1), with no information provided on the nature of the polymer breakage. Buchholz et al.26 showed that scission of high MW polymers occurs preferentially near the chain mid-point and for larger MW species (in turbulent flow), leading to a decrease in polydispersity as determined by gel permeation (size exclusion) chromatography.26 During HVHF, flow through perforations/fractures during the initial fracture will create high levels of pressures and shear rates, likely creating strain rates well in excess of 105 s−1, a flow regime that has yet to be investigated for the mechanical degradation of PAM.
The objective of this study was to first examine the mechanical degradation of high MW PAM after flow through a sharp contraction into very narrow capillaries at the high pressures/shear rates that would be expected during the HVHF of tight shale formations. In each case, the degree of degradation was evaluated using the change in polymer MW distribution quantified by size exclusion chromatography both before and after flow through narrow capillaries. The MW distribution of degraded polymer was then used to establish a scaling relationship with the applied shear rates. Second, mechanical degradation was compared to chemical degradation of PAM under HVHF chemical conditions (high temperature, mg L−1 level Fe2+ at pH < 4) in terms of MW distribution and chemical functional groups of degraded polymer. Furthermore, sequential and combined degradation experiments by the two mechanisms were performed and the degree of degradation was quantified. The results presented here provides a holistic view of PAM degradation throughout the HVHF process by both chemical and mechanical mechanisms.
This apparatus consists of a high precision metering pump (Quizix® Q5000-10 K, rated as 10
000 psi, 15 ml min−1 max flow rate, Chandler Engineering), PEEKsil® capillary tubing (SGE analytical service by Trajan Scientific and Medical, Australia) connected by EXP® 2 titanium hybrid Ti-LOK ferrule (#15-20-04932, Optimize Technologies, OR) and standard reducing union (# ZRU21 T, VICI Valco® Instruments, TX); all parts were rated at a pressure of at least 15
000 psi. The capillary tubing had a polymer outer sheath (polyether ether ketone, PEEK), a polyimide layer in the middle, and a fused silica lining inside to provide very low adsorption characteristics. Experiments were performed with capillaries having inner-diameters of 50 and 75 μm, with an outer-diameter of 1.5875 mm (1/16′′).
Experiments were conducted at constant flow rate (determined by timed collection of the outflow) with the pressure recorded using Quizix® PumpWorks software. Samples (20 mL) were collected from the system outflow (after pressure equilibration, roughly 10 min) for offline determination of the PAM MW distribution. Linearized flow rate and pressure data were plotted to calculate the power law fluid index n and consistency factor K, which were then used to calculate shear rate,
, where V is the mean flow velocity and R is the capillary radius. Characteristic strain rate that represents the extensional component was calculated as
that was previously developed for sharp-contraction capillary flow.11 Thus, the shear rate and strain rate both have the same dependence on the fluid velocity and capillary radius in this system, making it very difficult to separate out the contributions of shear versus elongational flow on the extent of degradation. Therefore, we use V/R as the independent variable to represent the overall deformation rate of the fluid under such geometry and was used to establish the scaling relationship between fluid strain rate and molecular weight reduction. Note that the both
v and
are linearly proportional to V/R.
v < 106 s−1), but there was more than one order of magnitude reduction in peak MW after flow into the capillary at a V/R = 1.5 × 106 s−1 (shear rate
v = 2 × 107 s−1) (Fig. 1A). All shear rates were calculated using the power law fluid index n = 1.008 ± 0.025 (τ = Kγn) determined from a log–log plot of pressure versus flow rate (Table S1†). This value of n suggests that the flow was nearly Newtonian at the very high shear rates examined in this work. In addition, the strength of extensional flow component was calculated as the characteristic strain rate (
); the shear and strain rate of flow experiments with 75 μm capillary was presented in Table S1.† The data for the peak MW for the 50 and 75 μm capillary diameters appeared to be very similar, although the same trend was also seen when plotting the peak MW versus the average flow velocity in the capillary as suggested by Jouenne et al.22 The relationship between resulting MW with V/R was plotted on a log–log graph, suggesting a correlation of the form:![]() | (1) |
−0.69). Similar power-law relationships have been reported for polystyrene solution in transient abrupt contraction flow,28 polyethylene oxide and polyacrylamide solution in turbulent pipe flow,7 where the scaling exponent was found to range between 0.36–1. Such correlation reflects the critical fluid strength that is needed for chain rupture under specific flow geometry. This can be better seen in Fig. 1B, which is re-plotted using the data in Fig. 1A as the percent degradation, defined as the reduction in the peak MW divided by the initial MW. There was no degradation for the experiments with V/R below 105 s−1, suggesting that there is a critical fluid strain (or stress) needed to initiate the scission of the polymer chain. The percent degradation drastically increased after flow into capillaries at high deformation rates (Fig. 1B), as evident from the size exclusion chromatographs (Fig. 1C). In addition, the breadth of the MW distribution decreased after mechanical degradation, consistent with the preferential scission of the larger MW species near the middle of the polymer chain.
Our data demonstrate that a stronger extensional flow (corresponding to a higher capillary deformation rate) is required to break a shorter polymer chain (low MW), which is consistent with previous studies suggesting a critical (minimum) polymer size for chain scission under given flow conditions.22,26 It was suggested that a larger polymer chain is more likely to be deformed under strain due to 1) decreased molecular mobility (characterized by relaxation time), 2) a higher capacity of storing elastic energy by strain accumulation.28 This further highlights the importance of the power law scaling relationship under such flow regime
. As a result, the highest level of reduction in both the peak MW and polydispersity occurs at the first passage of the polymer through the highly contracting capillary (Fig. 2C), which is likely to reflect the degradation during the fracture initiation phase during HVHF operations. Subsequent flow through the fracture, including entrance to branched fractures, are likely to have lower shear rates due to pressure loss and leak off during fracture flow;30,31 thus, the subsequent degradation would be much less than the breakage seen during the entrance to the initial fracture.
![]() | ||
| Fig. 3 A) Effect of mechanical and chemical degradation on PAM. “Mech” indicates solution with just polymer that passes through a 75 μm capillary at a V/R of 1.2 × 106 s−1; all the samples with “Chem” indicate solutions of polymer mixed with 2 ppm Fe2+ at a pH 3.5. The order of “Mech” and “Chem” indicates the order of the experiment. B) FTIR spectra of raw, chemically, mechanically, and combined degraded polymer shows an increase in the carbonyl groups only after chemical degradation (arrows). (C) Chromatographs of raw, mechanically, and chemically degraded polymer with similar peak MW suggest a stronger PDI-narrowing capability of mechanical degradation. The chromatograph of the chemically degraded polymer was extracted from a previous study where the polymer was degraded for 14 h in the presence of outcrop shale at 80 °C.27 | ||
The differences in chemical and mechanical degradation were further studied using attenuated total reflectance Fourier transform infrared spectroscopy (ATR-FTIR). Mechanically degraded PAM had a similar FTIR spectrum as compared to the original polymer. In comparison, the chemically degraded polymer showed a distinct signal associated with the carbonyl group (peak at 1720 cm−1 in Fig. 3B). The carbonyl group generated during chemical degradation is due to the β-scission of peroxyl polymer radicals subsequent to the oxygen radical attack on the polymer chain,27 a phenomenon that does not occur during the C–C bond breakage by mechanical forces.
The polydispersity index (PDI) of the PAM decreased significantly after either mechanical or chemical degradation (Fig. 3C). The PDI for each polymer was calculated as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) as determined from the size exclusion chromatographs using appropriate calibration curves (created with PAM standards having a range of molecular weights). We selected a chromatograph from a previous study of chemical degradation27 with similar peak MW to better visualize the PDI comparison for the various degradation mechanisms. Mechanical degradation led to a narrower molecular weight distribution (smaller PDI in Fig. 3C) compared to chemical degradation, consistent with the physical picture that mechanical forces lead to the preferential breakage of the larger MW polymers near the midpoint of the chain.26 In contrast, chemically generated free radicals are likely to attack randomly along the entire polymer chain length, irrespective of the initial polymer MW. Mechanical degradation is less effective in reducing the peak MW when it follows chemical degradation since much of the chemically-degraded PAM will have low MW (below the critical MW for polymer chain scission) and will thus be unaffected by the extensional flow. In contrast, chemical degradation will be highly effective in further degrading the PAM that has already been subjected to the extensional flow. Note that previous studies of chemical degradation yielded PAM with peak MW below 2 × 105 Da after 24 h exposure to Fe2+-generated hydroxyl radicals at low pH and high temperatures,20 which is well below the lowest MW seen in this study after multiple sequential mechanical degradation events.
v−0.69 established here.
In addition, shale formations with high ferrous-bearing minerals can utilize oxygen in the fluid to generate oxygenic radicals that can cause further chemical degradation of PAM. Combined chemical and mechanical degradation results also suggest distinct features of the two mechanisms which suggests that each mechanism is likely to dominate at different stages of fracturing events. Mechanical degradation is likely to be dominant at the entrance of fracture when polymer MW is still high (above critical chain length for scission) and chemical degradation is not fast enough to occur (milli-second for mechanical degradation versus minute to hour for chemical degradation). Once inside the fracture, mechanically degraded polymer chains are likely to be chemically degraded, where chain scission occurs randomly along the polymer chain, generating carbonyl groups via β-scission that are absent in both the raw and mechanically degraded polymer.
v ∼ 105–107 s−1;
∼ 105–4 × 106) unique to HVHF operations. Log–log scaling relationship between final MW of polyacrylamide and fluid deformation rate was developed
. This relationship enables the estimation of the maximal three orders of magnitude of MW reduction (with a starting MW of 107 Da) under a shear rate of 108 s−1. Mechanical degradation leads to a decrease in polydispersity of PAM suggesting preferred scission at mid-chain compared to random chain scission of chemical degradation. Furthermore, mechanically degraded PAM is chemically similar to un-degraded PAM, compared to carbonyl group generation during chemical degradation by β-scission of oxyl radicals. The combination of mechanical and chemical degradation introduces PAM with a wide range of MW distribution in the wastewater. Largely degraded polymer can contribute significantly to the polar organic fraction in the wastewater and enhance the likelihood of releasing hazardous acrylamide monomer into the environment. Polymer debris with low degree of degradation can significantly increase the fouling potential during the membrane treatment of the resulting wastewater. This work provides mechanistic insights into the unique transformation pathway of polyacrylamide in the deep subsurface and justify the need for more detailed chemical and toxicological analyses of degraded polymer products in HVHF wastewaters.
Footnote |
| † Electronic supplementary information (ESI) available: High shear rate capillary flow setup images, power law fluid parameters calculation, estimation of shear rates in actual hydraulic fracturing operations are included in the ESI. See DOI: 10.1039/c9ew00530g |
| This journal is © The Royal Society of Chemistry 2020 |