First published on 3rd September 2019
Aluminosilicate-based zeolite materials, such as ZSM-5 and mordenite, are well-studied as catalysts. Typical approaches to synthesize these zeolites require either templates or seeds to direct ordered crystal growth and both of these are expensive and add to the complexity of zeolite synthesis. In this paper, we describe a solvent-free and template-free method to synthesize crystalline ZSM-5 and mordenite zeolites without any added seed crystals. Key to the success of this approach is a mechanochemical precursor pre-reaction step. High-energy ball-milling is used to initiate a solid-state metathesis (exchange) reaction between Na2SiO3 and Al2(SO4)3 reagents, forming crystalline Na2SO4 and well-mixed aluminosilicate precursor. The solid precursor mixture is thermally converted to crystalline ZSM-5 or mordenite at moderate 180 °C temperatures without solvents or an organic amine structure directing template. Variations in Si/Al ratios in the precursor mixture and additions of solid NaOH to the mechanochemical reaction were found to influence the subsequent growth of either crystalline ZSM-5 or mordenite zeolites. The crystalline zeolites from this solvent-free and template free method have high ∼300 m2 g−1 surface areas directly from the synthesis without requiring high-temperature calcination. These materials are also comparably active to their commercial counterparts in cellulose and glucose biomass catalytic conversion to hydroxymethylfurfural.
Typically, crystalline zeolites are synthesized in the presence of structure-directing organic templates using solvothermal synthesis at relatively high temperatures and pressures for long times (170–230 °C, and 68–120 h).2,7–11 These templated solvothermal syntheses have several drawbacks including environmental waste issues related to the separation and disposal of aqueous solutions containing inorganic and organic species and energy-intensive issues related to subsequent high-temperature air calcination required to destructively remove the organic template form the internal pores of the product zeolite. The internal pore structure of a zeolite must be accessible for desired catalyst or separation activities.
There is ongoing interest in developing zeolite syntheses that are more sustainable and environmentally friendly, such as by eliminating or reducing the amount of required solvents or organic templates. For example, some studies report the aqueous solvothermal organic template-free synthesis of ZSM-5 and mordenite zeolites.1,5,12–20 The elimination of structure directing organic templates has been accomplished by judicious manipulation of inorganic components (e.g., Na, Al, Si) in the solution environment to facilitate zeolite nucleation and particle growth.5,18,21–23 Alternatively, crystalline zeolite nanoparticles have been used as growth seeds in solvothermal reactions instead of organic molecular templates. In solvothermal ZSM-5 zeolite synthesis, ZSM-5 seeds are added to the precursor solution and growth of the zeolite occurs on the surface of the seeds.24–27 We and others have reported the successful seed-assisted synthesis of ZSM-5, ZSM-11, beta, and mordenite zeolites.24,26,28–31 Some potential drawbacks of seed-assisted zeolite syntheses are that reactions still generate mixed inorganic/organic liquid waste and they also require the careful production and characterization of nanoparticle seeds prior to large scale zeolite synthesis.
Water or alcohols are typically used in solvothermal zeolite synthesis to enhance metal ion mixing and diffusion, leading to crystal growth. Solvents are at high temperatures near 200 °C and may generate high pressures during heating that require use of high pressure reaction vessels. The use and disposal of large amounts of solvent also increases the complexity of zeolite synthesis. To overcome potential solvothermal reaction issues, several studies describe solvent-free zeolite synthesis.32–41 Recently crystalline mordenite zeolite was produced by a solvent-free and template-free reaction at 200 °C with boehmite aluminum oxyhydroxide, Na2SiO3, and silicic acid.42
Our recent contribution to solvent-free ZSM-5 zeolite synthesis identified mechanochemically induced precursor reactions that enabled the successful synthesis of crystalline ZSM-5.32,43 We found that extended manual grinding of Na2SiO3·9H2O with NH4Cl produced crystalline NaCl via a solid-state exchange reaction and created a basic paste from NH4OH and freed waters of hydration. The inclusion of Al(OH)3 in the mixture led to well-mixed aluminosilicate reactants. An organic zeolite structure directing agent, tetrabutylammonium bromide (TBABr) was also part of the reagent mixture and was necessary for the successful growth of crystalline ZSM-5 in subsequent 160 °C solvent-free reactions. Calcination at 550 °C was required after synthesis to open the zeolite pore structure by removal of the embedded organic template.
Mechanochemical reactions have gained a strong foothold in recent years as a component of the organic and inorganic materials reaction toolbox and there are several examples of their use in synthesizing complex solid-state materials.44 For example, one recent study shows that lead-based mixed-halide solid-solution perovskites are produced using mechanochemical reactions between cesium halides and lead halides45 and another describes the formation of transition-metal porphyrins without solvent.46 The mechanochemical approach relies on the grinding force to destroy the crystalline structure of solid reagents. Small amounts of solvent or water may be added or released from hydrated forms of reagents during the grinding process. These solvent additives can facilitate reactions between starting materials and lead to the formation of intermediates and target materials.32,44,47,48
Given the success of mechanochemically assisted solvent-free zeolite synthesis, we examined alternate precursor combinations and hydroxide base modifications without organic amine or zeolite seed structure directing templates. This study reports our success with high energy ball milling that provides sufficient mechanochemical energy to achieve a reaction between Na2SiO3 and Al2(SO4)3 and yields crystalline Na2SO4 and an intimately mixed aluminosilicate precursor. Through alterations in Si/Al and Na/Al ratios in the precursor mixture, both crystalline ZSM-5 and mordenite zeolites are produced at 180 °C with high surface areas without requiring a high temperature calcination step. This work represents a rare example of zeolite crystal growth in the absence of solvent, organic structure directing agents, or zeolite seed crystals. These crystalline zeolites function as effective biomass catalysts analogous to their commercial analogs (e.g., glucose to hydroxymethylfurfural conversion).
The text, tables, and figure captions, generally report reagent ratios using conventional zeolite synthesis ratios, namely calculating ideal amounts of SiO2, Al2O3, and Na2O that could be produced by the precursor mixture. The calculated amount of SiO2 arises from both fumed SiO2 and Na2SiO3, Al2O3 arises from Al2(SO4)3, and Na is calculated as Na2O from both Na2SiO3 and NaOH (if applicable). In some cases, a value of “free” Na2O is calculated assuming that Na that forms Na2SO4 is unavailable for zeolite synthesis.
:
30 HCl
:
HF solution. The obtained suspension was sonicated for 10 min and after that, 6 mL of 5 vol% boric acid and 0.6 mL of concentrated nitric acid were added to complete dissolution. DI water was added to adjust the total volume to be 10 mL.
:
50 v/v acetonitrile
:
water at a flow rate of 0.8 mL min−1. The amount of hydroxymethylfurfural (HMF) present in the products was determined by an external standard curve based on the peak area of the HMF signal in the product versus standard solutions. The unreacted biomass was determined as isolated post-reaction solid mass minus the catalyst mass. The percent biomass conversion was calculated as the mass ratio of reacted biomass to initial biomass in the reactor. The yield of HMF was calculated as the ratio of HMF in the solution relative to the amount of initial biomass in the reactor.
Based on the high energy ball milling XRD results, 50 min of grinding likely results in a net mechanochemical pre-reaction consistent with that shown below in eqn (1).
| 3Na2SiO3·9H2O + Al2(SO4)3·18H2O → 3Na2SO4 + “Al2[SiO3]3” + 45H2O | (1) |
In our previous work, the reagent's waters of hydration were freed during mechanochemically induced NaCl formation.32,43 Since NaCl does not form extensive salt hydrates, the released water led to a distinct wet paste-like appearance for the ground precursor mixture. In contrast, the 50 min ground product from eqn (1) is still a free flowing powder, which is not surprising as Na2SO4 is a well-known drying agent with extensive hydration ability forming a stable decahydrate, which would tie up most of the reagent freed waters of hydration. In addition to the two reagents in eqn (1), fumed silica is used to produce specific Si/Al ratios that are used for zeolite growth. In addition, free sodium ions are needed for zeolite growth and these are supplied by additional Na2SiO3 and/or, as will be discussed later, through NaOH additions. In zeolite structures where Si4+ sites are replaced by Al3+, the addition of Na+ cations is also needed for charge balance.
While the 50 min high energy ball milling resulted in the most “complete” mechanochemical exchange reactions (Fig. 1A), and effective mixing of solid reagents, this may not necessarily lead to the successful solvent-free and organic template free thermal conversion to crystalline zeolites. Parallel solvent-free zeolite synthesis reactions were performed at 180 °C with solid precursor mixtures that were unground and subjected to 25 min or 50 min of high energy ball mill grinding. The 180 °C heating time was varied from 24 to 72 h and the isolated products after heating were washed with water to remove byproduct salts and soluble species. The XRD results from 24 h heating at 180 °C (Fig. 1B) clearly show that crystalline ZSM-5 is only produced from the 50 min ball milled reagent mixture. All of the crystalline peaks in Fig. 1B(c) correspond to ZSM-5 (PDF #00-037-0361), while the XRD patterns of both unground and 25 min ball milled samples are essentially amorphous. The relative crystallinity of the 24 h (50 min ball milling) product was about 68% and with a measured surface area of 198 m2 g−1. These values indicate that the ZSM-5 product after 24 h heating is not fully crystallized. Extended heating of the 50 min ball milled reagent mixture for 48 and 72 h results in improved crystallinity for ZSM-5 (Fig. 1C and D). The 48 h and 72 h ZSM-5 reaction products have relative crystallinities (surface areas) of 95% (324 m2 g−1) and 93% (311 m2 g−1), respectively. In contrast, the unground and 25 min ball milled mixture transform from amorphous materials to dense crystalline quartz rather than to porous aluminosilicate zeolites. These results indicate that the extended 50 min ball-milling pre-reaction that forms crystalline Na2SO4 also produces sufficiently mixed aluminosilicate intermediates that yield crystalline porous zeolite framework structures. Zeolite growth and crystallization at 180 °C takes place in the presence of a Na2SO4 salt that will release its waters of hydration during the reaction and they may influence zeolite crystallization and particle growth. This is a rare example of crystalline zeolite synthesis without any added solvent or organic molecular or zeolite seed structure directing templates.
The SEM images of the crystalline ZSM-5 products from 50 min ball milled mixtures also show a progression from irregular and incompletely formed particles after 24 h of heating to faceted ∼8 μm aggregated crystallites after 48 h and finally to fairly uniform ∼13 μm particles after 72 h of heating at 180 °C (Fig. 2). These microscopy results show that even in the absence of solvent or hydrothermal gel to crystallite transformations, the mechanochemically mixed reagents are sufficiently combined to grow into large organized faceted particles in the ten micrometer range.
In conventional zeolite synthesis, an organoamine structure directing template fills the zeolite pores and is removed by a high temperature air calcination step that then yields zeolites with high surface area. Since our reactions do not contain organic templates, a higher temperature air calcination is not required to access the internal zeolite pore structure. To examine the structural stability of our 180 °C synthesized materials, products from a 50 min ball mill pre-reaction followed by 180 °C heating for 24, 48, or 72 h were subsequently calcined at higher 550 °C temperatures in air. The XRD patterns for the calcined samples are shown in Fig. S2.† The sample from a 24 h synthesis was unstable and collapsed to a dense quartz phase after the calcination. On the other hand, samples from longer synthesis times (48 and 72 h) retained stable crystalline the ZSM-5 zeolite structure after calcination (Fig. S2†). These results are consistent with our recent work on a different mechanochemical ZSM-5 reaction where incomplete initial structure formation led to decomposition to dense silica after calcination.43
Sodium cations (Na+) have a charge balancing function for Al3+ substitution into silica-based zeolites. They also can play a role as a structure-directing agent to facilitate the growth of crystalline zeolites in the absence of an organic template directing agent.22,23 In our synthesis, Na2SiO3 is the sodium source and after grinding some sodium will be sequestered as Na2SO4. Several reagent mixtures with varying Na2SiO3 amounts were ball-milled for 50 min followed by 180 °C heating for 48 h to determine the influence of sodium content in the reagent mixture on the crystallinity of the zeolite product. The Na2SiO3, Al2(SO4)3, and SiO2 precursor mixtures corresponded to equivalent Na2O
:
Al2O3
:
SiO2 ratio of x
:
1
:
30, where x was varied from 3–9. Notice from eqn (1), that when x = 3, this corresponds to essentially all Na+ from Na2SiO3 being sequestered in the three Na2SO4 byproducts during the mechanochemical pre-reaction, thus there may be no “free” Na+ available for subsequent zeolite structure directing/templating. After thermal treatment, the x = 3 reaction resulted in an amorphous XRD pattern, but as the “free” sodium ion content increased, the growth of crystalline ZSM-5 is evident (Fig. 3). At the highest levels of excess sodium examined here (Na2O/Al2O3 = 9), a more aluminum-rich mordenite zeolite (PDF #00-011-0155) is crystallized instead of ZSM-5. Poorly crystalline ZSM-5 and mordenite are observed with a Na2O/Al2O3 = 7 reaction ratio. The growth of some crystalline ZSM-5 is evident even at low “free” sodium levels (Na2O/Al2O3 = 4) showing the value of well-distributed sodium cations present in the ball-milled and exchanged precursor mixture that allows zeolite structure direction from low sodium content in the absence of solvent or organic template.
A different approach to modify the sodium content in the precursor mixture was accomplished through the addition of solid NaOH to the reagent mixture consisting of Na2SiO3, SiO2, and Al2(SO4)3. In addition to providing a source of sodium, NaOH addition significantly alters the basicity of the resulting solid mixture, which can aid in metal hydroxide formation and condensation. The reagents were ball-milled for 50 min with varying amounts of NaOH to maintain the same Na/Al/Si ratios as used above (equivalent Na2O
:
Al2O3
:
SiO2 ratio of x
:
1
:
30, where x = 3–9). After 180 °C heating for 48 h, the washed products showed the XRD patterns in Fig. 4. One clear effect of NaOH-based sodium ion addition on basicity or reactivity is that the more aluminum-rich mordenite zeolite preferentially crystallizes over the ZSM-5 zeolite even for the same ratios (e.g., Na2O
:
Al2O3
:
SiO2 ratio of 5
:
1
:
30) that produced ZSM-5 as shown earlier (Fig. 3).
Given that a more aluminum-rich zeolite, mordenite, crystallizes in preference to ZSM-5 under several conditions of excess sodium ions where the Al2O3
:
SiO2 ratio was fixed at 1
:
30, a series of analogous mechanochemically mixed reactions were performed (180 °C, 48 h) using a higher silica ratio equivalent (Al2O3
:
SiO2 of 1
:
40) with fumed SiO2 added to increase the silica content. The XRD results of washed products are shown in Fig. S3 and S4.† Generally, without NaOH, the higher silica content yields essentially amorphous products until crystallization of a mixed ZSM-5/mordenite zeolite product at the highest sodium level (equivalent Na2O
:
Al2O3
:
SiO2 ratio of 9
:
1
:
40). When NaOH was used to modify the sodium content and basicity of the mechanochemically ground solid mixture of Na2SiO3, Al2(SO4)3, and SiO2, crystalline ZSM-5 forms at several higher sodium ratios (equivalent Na2O
:
Al2O3
:
SiO2 ratio of 7/8
:
1
:
40), while crystalline mordenite was not observed. Table 1 summarizes the XRD results observed for variations in reagents with and without addition of NaOH.
:
Al2O3
:
SiO2 ratios of x
:
1
:
y, where x = 3–9 and y = 30 or 40a
| Na2O/Al2O3 ratio | SiO2/Al2O3 ratio | |||
|---|---|---|---|---|
| 30 | 30 (with NaOH) | 40 | 40 (with NaOH) | |
| a Mechanochemically ground for 50 min, then thermally treated at 180 °C for 48 h, and then washed with water. The noted equivalent molar ratio amounts of SiO2 arises from both fumed SiO2 and Na2SiO3, Al2O3 equivalent arises from Al2(SO4)3, and Na2O is from both Na2SiO3 and NaOH (if applicable). | ||||
| 3 | Amorphous | Amorphous | Amorphous | — |
| 4 | Amorphous + trace ZSM-5 | Amorphous + trace ZSM-5 | Amorphous | Amorphous |
| 5 | ZSM-5 | Mordenite + quartz | Amorphous + trace ZSM-5 | Amorphous + trace ZSM-5 |
| 6 | ZSM-5 | — | Amorphous + trace ZSM-5 | Amorphous + trace ZSM-5 |
| 7 | ZSM-5 + mordenite | Mordenite | Amorphous + trace ZSM-5 | ZSM-5 |
| 8 | — | — | Quartz | ZSM-5 |
| 9 | Mordenite | Mordenite | Mordenite + trace ZSM-5, quartz | Quartz |
The solvent-free and organic template free reactions that successfully use high energy ball milling pre-reactions to produce single-phase ZSM-5 or mordenite zeolites are highlighted in bold in Table 1. Zeolite product phase formation was strongly influenced by the free Na content as crystalline zeolites do not form at low free sodium levels (amorphous, disordered products), ZSM-5 forms at moderate sodium levels, and mordenite is favored at the highest sodium levels. The alkaline basicity in the mechanochemically ground precursor mixture, may lead to better aluminosilicate mixing that leads to crystallization of ZSM-5 using higher silica ratios and to mordenite at lower sodium levels. Several of these single-phase zeolite products were examined in more physical and compositional detail below.
As noted earlier, the 48 h heating at 180 °C of mechanochemically mixed reagents with equivalent Na2O
:
Al2O3
:
SiO2 ratios of 5
:
1
:
30 leads to well-formed ZSM-5 crystallites near 8 μm in size (Fig. 2). Similarly well-formed aggregates of plate-like particles are observed for other single phase ZSM-5 products formed with NaOH and higher Si/Al ratios (Na2O
:
Al2O3
:
SiO2 ratios of 7
:
1
:
40 and 8
:
1
:
40). The increased silica content and inclusion of NaOH here only modestly affect the ZSM-5 crystallite shape or size as the elongated faceted particle slabs in Fig. 5A and B are about 5–6 μm in their longest dimension. In contrast, two single-phase mordenite products are shown in Fig. 5C and D, one with added NaOH and one without, and they both form larger particles than ZSM-5, approaching ∼10 μm along the longer slab direction. There are also indications of more uniform cube-like particle structures in the aggregates.
![]() | ||
Fig. 5 SEM images of single-phase ZSM-5 (A and B) or mordenite (C and D) zeolites synthesized from reagent mixtures of Na2SiO3, Al2(SO4)3, and SiO2 with and without NaOH addition (equivalent oxide amounts with Na2O : Al2O3 : SiO2 ratios of x : 1 : y, see Table 1 entries) that were mechanochemically ground for 50 min, then thermally treated at 180 °C for 48 h, and then washed with water. Equivalent metal oxide ratios are: (A) 7 : 1 : 40 (with NaOH), (B) 8 : 1 : 40 (with NaOH), (C) 9 : 1 : 30, and (D) 7 : 1 : 30 (with NaOH). | ||
Beyond crystalline phase and physical morphology, it is useful to compare the relative crystallinity of the zeolite products as well as their surface areas and elemental compositions. Table 2 shows comparison data for several single-phase ZSM-5 and mordenite products identified by XRD analysis. The ZSM-5 and mordenite products all show appreciably high relative crystallinity at or above 85% and total accessible surface areas near 300 m2 g−1, both of which are compare favorably to commercial crystalline zeolite standards (Table 2). It is important to reinforce that as opposed to zeolite syntheses that uses organoamine structure directing agents, these mechanochemically-assisted solvent-free reactions produce crystalline zeolites that do not require a high-temperature (∼500 °C) heating step to combust away embedded organic structure directing molecules and open up the internal zeolite channels and pores. The ICP-OES derived bulk compositions of the synthesized zeolites in Table 2 agree with typical Si/Al ratios for ZSM-5 and mordenite. The mordenite zeolite is the more Al-rich zeolite with Si/Al ratios between ∼5–12 while ZSM-5 materials have higher Si/Al ratios near or above ∼15.5 The single-phase ZSM-5 products here show higher Si/Al values of 12–17 versus mordenite products in the 6–7 range. Both solvent-free ZSM-5 and mordenite products contain higher sodium content (Na/Al ∼ 2–6) than the ideal Na/Al ≈ 1 values measured for commercial samples. The additional sodium may be a consequence of the concentrated solid-state growth process with some sodium serving a templating function as well as charge balance. For ZSM-5 samples, the addition of NaOH lead to larger sodium content in the final product. In the mixed phase and primarily amorphous isolated products, there is appears to be lower sodium incorporation, which may correlate with insufficient sodium content for effective zeolite templating (Table S2†).
| Samplesa | Precursor, Na2O : Al2O3 : SiO2b |
% Relative crystallinity | Surface area (m2 g−1) | Product composition, Na2O : Al2O3 : SiO2c |
|---|---|---|---|---|
a Sample names are denoted as: zeolite phase – Na2O/Al2O3 molar ratio in reaction. MOR = mordenite zeolite and “comm” refers to commercial sodium-containing zeolite samples.
b Equivalent metal oxide molar ratios in reactions are shown that arise from Na2SiO3, Al2(SO4)3, and SiO2 with and without NaOH addition. Note that ideally molar equivalents of Na are sequestered as Na2SO4, so “free” Na for reaction is lower (e.g., 5 : 1 : 30 would be 2 : 1 : 30 for free Na available).
c Relative molar ratios are based on bulk product compositions measured by ICP-OES analysis.
|
||||
| ZSM-5-5 | 5 : 1: 30 |
95 | 324 | 2.2 : 1.0 : 26 |
| ZSM-5-6 | 6 : 1: 30 |
90 | 307 | 1.7 : 1.0 : 24 |
| ZSM-5-7 | 7 : 1: 40 (with NaOH) |
94 | 318 | 5.8 : 1.0 : 33 |
| ZSM-5-8 | 8 : 1: 40 (with NaOH) |
89 | 298 | 4.9 : 1.0 : 31 |
| MOR-7 | 7 : 1: 30 (with NaOH) |
92 | 302 | 3.4 : 1.0 : 13 |
| MOR-9 | 9 : 1: 30 |
85 | 287 | 4.8 : 1.0 : 14 |
| Comm-Na-ZSM-5 | n/a | 100 | 361 | 0.93 : 1.0 : 37 |
| Comm-Na-MOR | n/a | 100 | 371 | 1.55 : 1.0 : 11 |
| Samplea | ICP composition, Na2O : Al2O3 : SiO2b |
Surface area (m2 g−1) | Biomass conversion (%) from glucose (cellulose) | HMF yield (%) from glucose (cellulose) |
|---|---|---|---|---|
| a Sample names are denoted as: zeolite phase – Na2O/Al2O3 molar ratio in reaction. MOR = mordenite zeolite and “comm” refers to commercial zeolite samples. b Relative molar ratios are based on bulk product compositions as measured by ICP-OES analysis. | ||||
| H-ZSM-5-5 | 0.27 : 1.0 : 33 |
320 | 83 (53) | 38 (30) |
| H-ZSM-5-6 | 0.30 : 1.0 : 29 |
311 | 72 (49) | 42 (24) |
| Comm H-ZSM-5 | 0.12 : 1.0 : 41 |
355 | 82 (65) | 48 (35) |
| H-MOR-7 | 0.44 : 1.0 : 12 |
296 | 76 (43) | 31 (27) |
| H-MOR-9 | 0.72 : 1.0 : 17 |
283 | 78 (40) | 36 (22) |
| Comm H-MOR | 0.23 : 1.0 : 13 |
373 | 88 (60) | 37 (28) |
Several crystalline acid-exchanged ZSM-5 and mordenite (H-ZSM-5 and H-MOR) materials were tested for the catalytic performance in the biomass conversion of both ground glucose and cellulose. In the absence of a catalyst, very low biomass conversions (HMF yield) of 21% (3%) and 13% (0.8%) were found for glucose and cellulose, respectively. Ground cellulose was tested with commercial ZSM-5 and mordenite zeolite catalysts and both showed good 60–65% total conversion with ∼28–35% HMF yields (Table 3). As expected, glucose conversion was higher than cellulose (∼80–90% with HMF yields near 40–50%). The acid-exchanged ZSM-5 and mordenite samples yield catalysis results generally about ∼10–15% lower than the commercial zeolite samples with total biomass conversion (HMF yield) ∼40–50% (∼20–30%) for cellulose and ∼70–80% (∼30–40%) for glucose (Table 3 and Fig. 6). The commercial zeolites have ∼40–80 m2 g−1 higher surface areas than the solvent-free template free zeolites, which will impact the number of surface catalytic sites. A qualitative examination of acid sites using pyridine surface reactions was performed on acid-exchanged commercial ZSM-5 and MOR versus several zeolites synthesized in this work. An IR analysis of pyridine exposed samples, shows qualitatively similar features consistent with a mixture of Lewis and Brønsted acid sites (Fig. S6 and S7†).55,56 The small differences in catalytic activity could be attributed to differences in aluminum content, surface area, and surface acidity. These results show that the zeolites synthesized by a mechanochemically-assisted mixing with salt forming pre-reaction followed by solvent-free and template-free synthesis have accessible pore structures and show comparable catalytic activity to commercial zeolites.
![]() | ||
| Scheme 1 Graphical summary of key reactions steps used and observed phase formation from mechanochemically-assisted solvent-free and template-free zeolite synthesis without using any seeds. | ||
Footnote |
| † Electronic supplementary information (ESI) available: Molar ratios of reagents used in mechanochemical reactions, ICP-OES results, additional powder XRD data, nitrogen adsorption–desorption isotherms, and IR data for pyridine-reacted zeolites. See DOI: 10.1039/c9na00399a |
| This journal is © The Royal Society of Chemistry 2019 |