Centre for Nanoscience and Nanotechnology, Department of Chemistry, The Gandhigram Rural Institute – Deemed to be University, Gandhigram-624 302, Dindigul, India. E-mail: abrajohn@yahoo.co.in; s.abrahamjohn@ruraluniv.ac.in; Fax: +91 451 245 3031; Tel: +91 451 245 2371
First published on 10th May 2018
In this paper, a new galvanic displacement reduction (GDR) approach was demonstrated for Au–PtNPs synthesis with different Pt
:
Au compositions in an aqueous medium. PtNPs were initially synthesized by the reduction of H2PtCl6 using trisodium citrate and sodium borohydride. Addition of various concentrations of HAuCl4 to PtNPs leads to the formation of Au–PtNPs, which follows the GDR between Pt(0) and AuCl4− ions. The formation of Au–PtNPs was monitored by UV-vis spectroscopy by tuning the mole ratio of Pt
:
Au. HR-TEM images showed that the Au–PtNPs were spherical with 11 nm diameter. HR-TEM, XRD and XPS analysis showed that the formed Au–PtNPs were in the form of a core–shell structure. The colloidal Au–PtNPs were then attached on a glassy carbon (GC) electrode via a 1,6-hexanediamine linker for the methanol oxidation reaction (MOR) and oxygen reduction reaction (ORR). The attachment of Au–PtNPs was further confirmed by XRD, line scanning coupled with energy-dispersive X-ray spectroscopy (EDS) and cyclic voltammetry (CV). The Au–PtNPs modified electrode exhibits a higher heterogeneous electron transfer rate constant of 4.12 × 10−3 cm s−1 than bare (1.01 × 10−4 cm s−1) and PtNP (1.77 × 10−4 cm s−1) modified GC electrodes. Further, the Au–PtNPs modified electrode exhibited a composition dependent activity towards the MOR and ORR. It was found that the modified electrode with a Pt
:
Au ratio of 1
:
0.09 shows 8 times more sensitive oxidation for the MOR when compared to a commercial Pt/C catalyst. The present Au–PtNPs catalyst exhibits a greatly enhanced catalytic activity in terms of mass activity (132 mA mg Pt−1) and excellent stability relative to the commercial Pt/C catalyst.
Direct alkaline alcohol fuel cells have been investigated over the past decade due to their faster kinetics for alcohol oxidation and the oxygen reduction reaction (ORR) in alkaline solutions, higher power generation efficiency, easy handling of liquid fuels and low emission of pollutants.6–12,17 Similarly, methanol fuel cells are promising energy conversion devices because of their high energy density, low operating temperature, low pollutant emission, easy storage and transportation of fuels, and high conversion efficiency.6–10,17–20 Even though Pt catalysts are well known for methanol oxidation due to their surface binding properties, there are a few critical issues faced by them which include sluggish kinetics and poor stability besides high cost.18–20 Since CO is very sensitive to the surface binding properties, it strongly binds with the active sites of the Pt catalyst completely poisoning the active surface.21 To remove CO from the surface of PtNPs, the formation of Pt–OH is very essential (eqn (1) and (2)), but it occurs only at high potential.22
| Pt–CH2O → Pt–CO + 2H+ + 2e− | (1) |
| Pt–CO + Pt–OH → 2Pt + CO2 + H+ + e− | (2) |
Hence, designing an alternate catalyst or modifying the Pt catalyst is highly essential to sort out the above problems. Moreover, it is essential to reduce the cost of the Pt catalyst for a sustainable commercialization of fuel cells. Combining Au with Pt as BMNPs can overcome the disadvantages of the Pt catalyst, and the presence of Au provides a platform for the oxidation of poisonous intermediates such as CO by changing the electronic band structure and activation energy.6–10 Further, the Au–OH formation is facile in the Au-based catalyst in contrast to the Pt catalyst.8–10,23 It has already been reported that Au–PtNPs have higher catalytic activity than Pt but they depend on the composition of Pt and Au.6–10,24 The availability of the free Pt surface in the Au–Pt assembly would be expected to enhance the oxidation of methanol.
It has already been shown that Au–PtNPs serve as a strong platform for methanol oxidation.6–10,24 Several methods have been reported in the literature for the synthesis of Au–PtNPs which include co-reduction,25 sonication, wet chemical synthesis,26 seed mediated synthesis,9,27 two phase synthesis28 and the galvanic displacement reaction (GDR).29,30 Among these methods, the GDR method gains considerable attention due to its ease of handling, cost effectiveness, high throughput and simple experimental set up.29,30 The electroless mechanism is the basis of the GDR in which the reduction of metal ions to metal NPs is favoured without a reducing agent as well as external electric current.16,29–31 Very recently, Engelbrekt et al. prepared Au@PtNPs by GDR-like synthesis. They first prepared AuNPs by the chemical reduction of HAuCl4 in buffered glucose-starch solution at 95 °C and then added various concentrations of H2PtCl6 to prepare AuNPs to form Au@PtNPs. The resultant Au@PtNPs were mixed with graphitized carbon black for electrocatalytic applications.32 The present study provides a facile approach for the synthesis of Au@PtNPs in an aqueous solution as well as their fabrication on an electrode surface for electrocatalytic applications.
In the present study, the synthesis of Au–PtNPs in the solution phase by a galvanic displacement reaction and their application as a catalyst for methanol oxidation and oxygen reduction were described. Citrate capped PtNPs were initially prepared by a wet chemical method, and then various concentrations of HAuCl4 were added to them to form Au–PtNPs. The formation of Au–PtNPs follows the GDR between Pt atoms and AuCl4− ions which is mainly due to the difference in the thermodynamic potential. The as prepared Au–PtNPs were characterized by UV-vis spectroscopy, high resolution transmission electron microscopy (HR-TEM), X-ray diffraction (XRD) and X-ray photoelectron spectroscopy (XPS). Further, Au–PtNPs were fabricated on a glassy carbon (GC) electrode using 1,6-hexanediamine (HDA) as a linker for the electrochemical oxidation of methanol and the reduction of dioxygen.
000 rpm), and then the particles were separated. They were repeatedly washed with water and dried in a vacuum. The dried Au–PtNPs powder was used for XRD measurements. Scanning electron microscopy (SEM) measurements were carried out on a VEGA3 TESCAN, USA. Energy-dispersive X-ray spectroscopy (EDS) and line scan analysis were carried out using a Bruker Nano, Germany. For SEM, XRD, EDS and line scanning measurements, ITO plates were used as substrates with a similar modification to that used for the GC electrode.
:
Au mole ratio of 1
:
0 does not show any absorbance band in the visible region (Fig. 1, curve a) whereas on changing the mole ratio to 1
:
0.03, a new band appeared at 545 nm corresponding to the AuNPs suggesting the formation of Au–PtNPs (Fig. 1, curve b). On further increasing the mole ratios to 1
:
0.06 and 1
:
0.09, the SPR band intensity increased concomitantly (Fig. 1, curves c and d) and attained saturation at a 1
:
0.09 ratio, and further increment in the mole ratio to 1
:
0.12 does not affect the SPR (Fig. 1, curve e). In addition, the color of the solution gradually turns to reddish brown from brownish yellow upon the addition of HAuCl4 to the PtNP solution (Fig. 1, inset). The obtained spectral and color changes clearly suggest the successful formation of Au–PtNPs.
| 3Pt(s) + 2AuCl4− → 2Au(s) + 3Pt2+ + 8Cl− | (3) |
:
Au mole ratio of 1
:
0.09. The HR-TEM image of the PtNPs shows that the formed PtNPs were spherical in shape, and they were aligned to form chain like structures (Fig. 2A). The average particle size of the formed PtNPs was found to be ∼4 nm (Fig. S2A†). On the other hand, the HR-TEM image of Au–PtNPs shows elongated spherical particles (Fig. 2B) with an average size of ∼11 nm (Fig. S2B†). The increase in the particle size suggests the formation of Au–PtNPs. Further, lattice images of a single crystal are shown with different magnifications (Fig. 2C and D), clearly suggesting that the formed Au–PtNPs were in the form of core–shell NPs. Further, they show a hollow structure which was covered with another layer, maybe the holes generated by the PtNPs, and the reduced AuNPs may be placed inside the holes to form core–shell Au–PtNPs (Au@Pt core@shell NPs). The selected area electron diffraction patterns of Pt and Au–PtNPs show discrete dots, illustrating the crystalline nature of Pt and Au–PtNPs (Fig. S3A and B†). The obtained features again confirmed that the crystallinity of the PtNPs was not affected after the formation of Au–PtNPs.
Fig. 3 shows the XRD pattern of Au–PtNPs with a Pt
:
Au mole ratio of 1
:
0.09. It illustrates diffraction features at 38.17°, 44.34°, 64.52°, 77.48° and 82.10° corresponding to (111), (200), (220), (311) and (222) planes, respectively (JCPDS card no. 03-065-2870). Among these, the peak corresponding to the (111) plane is more intense than those corresponding to the other planes. The ratio between the intensity of the (200) and (111) diffraction peaks is much lower, indicating that the (111) plane is a predominant orientation. The width of the (111) peak was employed to calculate the average crystallite size of the Au–PtNPs using the Scherrer equation.35 The calculated average size of Au–PtNPs is 14 nm, which closely matches with the particle size obtained from HR-TEM. Besides, compared with Au (111), the peak intensity of Pt (111) is much higher, implying the Au (core)–Pt (shell) orientation.
![]() | ||
| Fig. 4 XPS obtained for Au–PtNPs: (A) survey spectrum and (B) deconvoluted Au 4f and Pt 4f regions of Au–PtNPs (inset A: enlarged survey spectrum). | ||
The morphology of the Au–PtNPs modified substrate with a Pt
:
Au mole ratio of 1
:
0.09 was characterized by SEM. Fig. S4† shows the SEM image obtained for the Au–PtNPs modified substrate. It shows that the attached Au–PtNPs were spherical in shape, and their size was found to be ∼20 nm. It also illustrates that the particles were distributed throughout the surface uniformly. Further, the Au–PtNPs modified substrate was characterized by XRD. Fig. 5A shows the XRD pattern obtained for substrates modified with Au–PtNPs with a Pt
:
Au mole ratio of 1
:
0.09. It shows diffraction features at 38.17°, 44.34°, 64.52° and 77.48° corresponding to the (111), (200), (220) and (311) planes of Au–PtNPs (JCPDS card no. 03-065-2870) (Fig. 5A, inset). It was found that there is no change in the crystalline planes. This suggests that the crystalline nature of the formed Au–PtNPs remains the same after being fabricated on the substrate. Among these, the peak corresponding to the (111) plane is more intense than those corresponding to the other planes. The ratio between the intensity of the (200) and (111) diffraction peaks was much less, indicating that the (111) plane is a predominant orientation. In addition, four characteristic peaks for Au–PtNPs marked by their indices ((111), (200), (220), and (311)) indicated that the resultant bimetallic nanoparticles have a face centered cubic (fcc) structure.30,31
![]() | ||
| Fig. 5 (A) XRD obtained for the Au–PtNPs modified substrate (* peaks correspond to the ITO substrate) (inset: JCPDS file of Au–PtNPs) and (B) EDS line spectra of the Au–PtNPs modified substrate. | ||
Fig. S5† shows the EDAX spectra of PtNPs, AuNPs and Au–PtNPs with a Pt
:
Au mole ratio of 1
:
0.09. The EDAX spectra of Pt and AuNP modified substrates show peaks at 2.050 and 9.442 keV corresponding to Pt and 2.21 and 9.71 keV corresponding to Au along with carbon, nitrogen and oxygen at 0.27, 0.39 and 0.53 keV, respectively (Fig. S5A and B†). On the other hand, the Au–PtNPs modified substrate shows both Pt and Au peaks, which confirms the successful modification of the Au–PtNPs (Fig. S5C†). It was found that the Pt and Au weight percentages of Au–PtNPs with a Pt
:
Au ratio of 1
:
0.09 are 7.23 and 4.17%, respectively. The Au–PtNPs with a Pt
:
Au mole ratio of 1
:
0.09 were further characterized by line scanning analysis.
Qualitative information on elemental distributions can be obtained by line-scanning analysis on the EDS analyzer, in which the diffusion profile of elements at an interface can be plotted as the number of X-ray quanta being counted vs. the spatial location along a line. Further, the normalised intensity scales simply make comparison of major and minor elements. Hence, it is a very much useful tool for the characterization of the bimetallic system.31Fig. 5B shows the line spectra of the Au–PtNPs modified substrate with a Pt
:
Au mole ratio of 1
:
0.09. It confirms that the particles present on the substrate were Au–PtNPs, and the intensity of PtNPs (Fig. 5B green line) was higher than that of AuNPs (Fig. 5B red line), implying that the AuNPs were covered with PtNPs. This clearly demonstrates that the PtNPs were in the outer shell, and the AuNPs were in the inner core. Hence, it is proposed that the formed Au–PtNPs were in the form of the Au(core)@Pt(shell) structure.
:
0.09 ratio.
In order to investigate the conducting nature of the Au–PtNPs electrode, an EIS study was carried out. Fig. 7 shows the Nyquist plots obtained for electrodes modified with GC/HDA/PtNPs, GC/HDA/AuNPs and GC/HDA/Au–PtNPs with a Pt
:
Au mole ratio of 1
:
0.09 in 1 mM K3[Fe(CN)6] containing 0.2 M PB solution (pH 7) at scanning frequencies from 0.01 to 100
000 Hz. A Randles circuit model [RS(CPE − RCT)] (Fig. 7, inset) was used to fit the impedance spectral data where RS refers to the solution resistance and CPE refers to the constant phase element. The charge transfer resistance (RCT) can be calculated from the semicircle obtained in the Nyquist plot, and it can control the interfacial electron-transfer rate of the redox probe between the solution and the electrode. The bare GC electrode shows a charge transfer resistance (RCT) value of 37.77 kΩ (curve a), whereas the AuNP and PtNP modified GC electrodes exhibit 25.89 and 21.47 kΩ, respectively (curves b and c). On the other hand, the Au–PtNPs modified electrode drastically reduced the RCT value to 16.34 kΩ (curve d). The increase in the conductivity of the Au–PtNPs modified electrode is mainly due to the higher surface homogeneity of the bimetallic system when compared to its respective monometallic counterparts. The obtained RS, C, and RCT values are given in Table S1.† The heterogeneous electron-transfer rate constant (ket) was calculated using eqn (4).31
![]() | (4) |
:
Au mole ratios in 1.0 M KOH at a scan rate of 50 mV s−1. The Au–PtNPs modified electrode does not show any response in the absence of methanol (Fig. 8, dotted line), indicating that this electrode is inert in this potential window. In the presence of methanol, the PtNP modified electrode shows an oxidation peak at −0.15 V (Fig. 8, curve a). When the AuNPs were blended with PtNPs in the form of Au–PtNPs with a Pt
:
Au mole ratio of 1
:
0.06, the oxidation peak current of methanol was dramatically enhanced by 6-fold, suggesting that Au–PtNPs act as a better catalyst when compared to PtNPs alone (Fig. 8, curve b). Moreover, it exhibits two oxidation peaks on the forward as well as the reverse scan. It is well known that the sharp current ramp in the forward scan can be ascribed to the characteristic methanol oxidation on the electrode surface, forming adsorbed carbonaceous intermediates such as CO and HCO−, which will be oxidized at higher potentials due to the formation of Au–OH species.6–10,26,27 In the reverse scan, desorption of OH-ads or reduction of Au-oxides regenerates the active metallic Au surface which allows further oxidation of methanol molecules at lower potentials. Further varying the Pt
:
Au mole ratio to 1
:
0.09, the oxidation peak current was enhanced (Fig. 8, curve c), and it decreased at a ratio of 1
:
0.12 (Fig. 8, curve d), indicating that the Pt
:
Au ratio of 1
:
0.09 is a suitable composition for the oxidation of methanol.
The forward peak current densities of the PtNP and Au–PtNPs catalysts with different mole ratios are shown in Fig. S7.† It can be seen that the current density (A m−2) of the Au–Pt catalyst increases with the increase of the Pt
:
Au ratio from 1
:
0 to 1
:
0.09 and decreased on further increasing the Au content in the Au–PtNPs assembly. The obtained maximum electrocatalytic activity of the Au–PtNPs catalyst (6.52 A m−2) with a Pt
:
Au ratio of 1
:
0.09 is about 7-fold higher than that of the PtNP catalyst (1.12 A m−2). The order of the catalytic activity of the prepared PtNPs and Au–PtNPs towards methanol oxidation is as follows: Au–PtNPs (Pt
:
Au = 1
:
0.09) > Au–PtNPs (Pt
:
Au = 1
:
0.06) > Au–PtNPs (Pt
:
Au = 1
:
0.12) > PtNPs (Pt
:
Au = 1
:
0).
The catalytic activity of the Au–PtNPs (Pt
:
Au = 1
:
0.09) modified electrode was further compared with that of the commercial Pt40/C catalyst. For this, a large volume (500 ml) of Au–PtNPs (Pt
:
Au = 1
:
0.09) was synthesized, centrifuged (10
000 rpm), washed with water and then dried in a vacuum. The dried Au–PtNPs powder was dispersed in water (1 mg/0.5 mL), and 30 μL of the solution was drop-cast on the electrode surface and dried overnight. The same amount of commercial Pt/C (30 μL of 1 mg/0.5 mL) was coated on the GC electrode with a similar procedure. The Au–PtNPs loading level on the GC electrode is 0.86 mg cm−2. Fig. 9A shows the CVs obtained for 1.0 M methanol in 1.0 M KOH at commercial Pt40/C and Au–PtNPs (1
:
0.09) modified GC electrodes at a scan rate of 50 mV s−1. The Pt/C modified electrode shows methanol oxidation at −0.20 V (curve a) whereas the Au–PtNPs modified electrode shows its oxidation at +0.23 V with an 8-fold higher oxidation current (curve b). The electrochemically active surface area (ECSA) of the Pt/C and Au–PtNPs modified electrodes can be calculated from the Coulomb charge for hydrogen adsorption and desorption (QH) in the negative-going potential scan, carried out at a scan rate of 10 mV s−1 using the following equation:7,8
![]() | (5) |
The transportation characteristics of methanol at the Au–Pt (Pt
:
Au–1
:
0.09) modified electrode were investigated by varying the scan rate in 1.0 M KOH, and the results are shown in Fig. S8.† While increasing the scan rate from 10–100 mV s−1, the anodic peak current increased. The relationship between the anodic peak current and the square root of scan rate is linear with a correlation coefficient of 0.9991 (Fig. S8,† inset), indicating that the electrochemical oxidation of methanol at the GC/Au–PtNPs electrode is a diffusion controlled process.
The obtained electrocatalytic activity of the PtNP and Au–PtNPs modified electrodes towards methanol oxidation can be explained as follows.26,27,32 The advantage of the core–shell structure is the possibility of coating the Au layer with the electrochemically active Pt thin layer. The efficiency of the electrocatalytic reaction strongly depends on the proximity of the reactant and the catalyst employed in the reaction. When the Pt content is high in the Au–Pt catalyst or completely Pt, it is difficult to form Pt–OH at lower potentials, and hence the electrocatalytic activity will be affected. Moreover, a thicker Pt layer will not allow methanol into the inner part of the material, and hence the formation of Au–OH is not possible. On the other hand, the AuNPs present in the Au–PtNPs assembly can catalyze poisonous intermediates such as CO that were absorbed on the active sites of PtNPs significantly, which results in the increased electrocatalytic activity of Au–PtNPs with the increase of Pt
:
Au mole ratio. These factors make the Au–PtNPs a suitable candidate for the electrochemical oxidation of methanol. On the other hand, AuNPs are not able to catalyze methanol, and thus, the electrocatalytic activity decreases at a higher Au content.
Further, the long-term stability of the prepared Au–PtNPs catalyst was examined towards the oxidation of methanol. Fig. 9B shows the amperometric i–t curve obtained for the oxidation of 1.0 M methanol at PtNP and Au–PtNPs modified electrodes in 1.0 M KOH at an applied potential of +0.6 V for 4000 s. It can be seen that the oxidation current of methanol at the Au–PtNPs modified electrode decreases gradually with the extension of time. After 100 s, the oxidation current remains unchanged, suggesting that the prepared Au–PtNPs modified electrode is highly stable towards the oxidation of methanol. It also exhibits higher stability and electrocatalytic activity than the Pt/C catalyst (Fig. 9B). The stability of the Au–PtNPs catalyst was also examined using a CV accelerated test. Fig. S9† shows CVs obtained for 1.0 M methanol at Pt/C and Au–PtNPs modified GC electrodes in 1.0 M KOH at a scan rate of 50 mV s−1. The Pt/C catalyst exhibits a stable electrochemical response towards methanol even after 100 cycles (Fig. S9,† curves a and a′). Even though, the prepared Au–PtNPs catalyst showed a slight shift in the oxidation potential of methanol, it exhibits higher oxidation current than the Pt/C catalyst (Fig. S9,† curves b and b′). The onset potential of the Au–PtNPs catalyst shifts positively by only 20 mV after the CV accelerated test, which is insignificant. The highest peak current density after potential cycling indicates that the catalyst not only possesses enhanced catalytic activity but also reveals considerable stability in the MOR.
The performance of the present modified electrode towards methanol oxidation was compared with those of the reported Au–Pt catalyst modified electrodes (Table 1).7,9,27,32,36 It can be seen from Table 1 that the Au–PtNPs prepared in the present study showed an 8-fold higher oxidation current with a less positive potential (+0.23 V) for methanol oxidation when compared to the commercially available Pt/C catalyst. Even though the Pt–Au string bead nanochain network modified GC electrode showed higher oxidation current for methanol oxidation its oxidation occurs at a more positive potential (+0.86 V). The excellent long-term stability of the Au–PtNPs catalyst further signifies that they can act as a suitable candidate in direct methanol fuel cells (DMFCs).
| S. no. | Electrodes | Oxidation potential (vs. SCE) | Medium | Mass activity (mA mg Pt−1) | Comparison with commercial Pt/C (oxidation current) | Ref. |
|---|---|---|---|---|---|---|
| a Multi-walled carbon nanotubes. b Potential is converted into a SCE potential. | ||||||
| 1 | Au–PtNPs/ITO | +1.03 V | 0.5 M H2SO4 | — | 2.5-Fold higher | 7 |
| 2 | Au–PtNPs/GCE | +0.68 V | 0.5 M H2SO4 | 161.6 | 6-Fold higher | 9 |
| 3 | Au–Pt honeycomb/GCE | +0.45 V | 0.5 M H2SO4 | 148.5 | 1.6-Fold higher | 27 |
| 4 | Au@PtNPs/GCE | +0.54 V | 0.1 M H2SO4 | 219 | 2-Fold higher | 32 |
| 5 | Au@PtNPs/MWCNTsa/GCE | −0.32 V | 0.5 M KOH | — | 3.5-Fold higher | 36 |
| 6 | Au@PtNPs/GCE | +0.18 Vb | 1.0 M KOH | 132 | 8-Fold higher | This work |
| O2 + 4H+ + 4e− → 2H2O | (6) |
| O2 + 2H+ + 2e− → H2O2 | (7) |
| H2O2 + 2H+ + 2e− → 2H2O | (8) |
Fig. 10 shows the CVs obtained for the ORR at bare GC, GC/HDA/PtNP and GC/HDA/Au–PtNPs electrodes with different mole ratios in oxygen saturated 0.5 M H2SO4 at a scan rate of 50 mV s−1. At the bare GC electrode, the ORR occurs at −0.46 V (Fig. 10, curve a). For the PtNP modified GC electrode, the ORR was obtained at −0.05 V which is a 410 mV more positive potential shift in the reduction potential when compared to the bare GC electrode (Fig. 10, curve b). On the other hand, when the Au–PtNPs with a Pt
:
Au mole ratio of 1
:
0.06 were modified on the GC electrode, the ORR current increased with a 100 mV more positive potential shift (Fig. 10, curve c). Interestingly, the Au–PtNPs with a Pt
:
Au mole ratio of 1
:
0.09 drastically enhanced the ORR current with a 150 mV more positive potential shift compared to the PtNP catalyst and a 660 mV more positive potential shift compared to the bare GC electrode (Fig. 10, curve d). Further, with increasing the Au content in the Au–PtNPs assembly to 1
:
0.12 mole ratio of Pt
:
Au, the ORR current decreased (Fig. 10, curve e). The obtained results suggest that the Au–PtNPs act as a suitable catalyst for the ORR, and the catalytic activity depends on the Au content.
The ORR was also carried out at the Au–PtNPs modified electrode using a rotating disc electrode (RDE). Fig. 11A shows linear sweep voltammograms obtained for the Au–PtNPs modified electrode in O2 saturated 0.5 M H2SO4 with the electrode rotation rates from 100 to 1600 rpm at a scan rate of 5 mV s−1. A gradual increase in the limiting current was observed while increasing the rotation rate owing to the increase in the mass transport to the electrode surface (Fig. 11A). The observed current density is normalized to the geometric area of the electrode in the respective curves. According to the Koutecky–Levich equation (eqn (9)), the inverse of current density could be given as the sum of the inverses of the above current components. It could also be given in terms of jk, B and ω expressed in revolutions per minute (rpm).
| 1/j = 1/jk + 1/Bω1/2 | (9) |
| B = 0.2nFCO2(DO2)2/3ν−1/6 | (9a) |
485 C mol−1), CO2 is the bulk concentration of oxygen (1.1 × 10−6 mol cm−3), DO2 is the diffusion coefficient of oxygen in sulfuric acid (1.4 × 10−5 cm2 s−1) and ν is the kinematic viscosity of sulfuric acid (1.0 × 10−2 cm−2 s−1).41,42 The Au–PtNPs modified electrode (Fig. 11B) shows a linear relationship of j−1vs. ω−1/2. The slope (B) of the straight line of the K–L plot could be used to calculate the number of electrons involved in the ORR. The Au–PtNPs modified electrode shows a B value of 12.39 × 10−2 mA−1 cm−2 rpm−1/2, and its corresponding n value is 4.3. The theoretical B value calculated for the 4-electron transfer process is 10.6 × 10−2 mA−1 cm−2 rpm−1/2.41 The experimental B and n values closely match with the theoretical values. This confirms that the Au–PtNPs modified electrode follows a 4-electron pathway for the reduction of oxygen as shown in eqn (6).
:
Au, and the formed Au–PtNPs were characterized by UV-vis spectroscopy. The newly appeared SPR band at 545 nm confirmed the formation of Au–PtNPs by the GDR. HR-TEM, XRD, XPS and line spectra results confirmed that the formed Au–PtNPs were in the form of the Au(core)–Pt(shell) nanostructure. The as prepared Au–PtNPs were fabricated on a GC electrode using HDA as a linker, and the modification was confirmed by SEM, XRD, EDS, CV and EIS. The Au oxide formation and reduction and Pt oxide formation and reduction peaks in the cyclic voltammograms again confirmed the successful fabrication of Au–PtNPs on the electrode surface. Further, the Au–PtNPs modified electrode exhibited composition dependent electrocatalytic activity towards methanol oxidation and the ORR. The Au–PtNPs modified electrode with a Pt
:
Au mole ratio of 1
:
0.09 showed higher electrocatalytic activity by showing 7-fold higher oxidation and 2.5-fold higher reduction currents towards methanol and the ORR, respectively, than the electrodes modified with bare GC, PtNPs and Au–PtNPs with other mole ratios. The Au–PtNPs prepared from this work showed methanol oxidation at +0.23 V with an 8-fold higher oxidation current when compared to the commercially available Pt/C catalyst besides long term stability. Thus, Au–PtNPs can be used as a suitable catalyst for methanol oxidation and the ORR.
Footnote |
| † Electronic supplementary information (ESI) available: Experimental details, UV-vis spectra of Au and PtNPs, histograms of HR-TEM images, SAED patterns, SEM image, EDAX spectra and CVs obtained for Au–PtNPs and methanol oxidation comparison and impedance spectral data of Au–PtNPs. See DOI: 10.1039/c7se00565b |
| This journal is © The Royal Society of Chemistry 2018 |