Ag nanoparticle decorated MnO2 flakes as flexible SERS substrates for rhodamine 6G detection

Yan Zhanga, Rui Jia Liub, Xiaofei Mac, Xiao Ying Liud, Yu Xin Zhang*a and Jie Zhang*b
aState Key Laboratory of Mechanical Transmissions, College of Materials Science and Engineering, Chongqing University, Chongqing 400044, P. R. China. E-mail: zhangyuxin@cqu.edu.cn
bThe Key Laboratory of Optoelectronic Technology & System, Education Ministry of China, Chongqing University, Chongqing 400044, P. R. China. E-mail: zhangjie@cqu.edu.cn
cChina Academy of Space Technology (Xi'an), Xi'an 710000, P. R. China
dEngineering Research Center for Waste Oil Recovery Technology and Equipment of Ministry of Education, College of Environment and Resources, Chongqing Technology and Business University, Chongqing 400067, China

Received 19th September 2018 , Accepted 24th October 2018

First published on 9th November 2018


Abstract

Smart design of advanced substrates for surface-enhanced Raman scattering (SERS) activity is challenging but vital. Herein, we synthesized a new kind of AgNPs/MnO2@Al flexible substrate as a SERS substrate for the detection of the analyte rhodamine 6G (R6G). The fabrication of porous MnO2 nanoflakes on Al foil was conducted via a facile hydrothermal strategy. Owing to the large active surface area of the MnO2 nanoflakes, the Ag nanoparticles were immobilized and displayed superior SERS performance with a low detection concentration of 1 × 10−6 M for R6G. In addition, the SERS performance was found to be strongly related to the morphology of the MnO2@Al substrate material. Our smart design may provide a new method of construction for other advanced SERS substrates for the detection of R6G.


1. Introduction

Surface-enhanced Raman spectroscopy (SERS) is a powerful and extremely sensitive analytical technique, which has attracted wide attention since it was first used to observe a rough Ag electrode.1 Until now, it has been intensely explored for use in many areas including biodetection, biomedicine, environmental monitoring, analytical chemistry, and so forth.2–6 Recently semiconductor nanostructures have been found to show the potential for SERS enhancement.7,8 Many researchers have proved that synthesized semiconductor–noble metal nanocomposites possess obvious Raman enhancement effects. For example, Zhao et al. fabricated a MoS2 nanosheet-silver nanoparticles composite for the detection of 2-mercaptobenzimidazole (MBI) molecules.9 Yang et al. synthesized an Ag-coated Fe3O4 microsphere using the solid-phase method, which was used to detect 4-aminothiophenol with a low concentration of 1.0 × 10−12 M.10 In addition, a noticeable increase in the Raman activities of molecules adsorbed onto Au–SiO2,11,12 Au–TiO2,13 Ag–CuO14 Ag-carbon,15 has also been reported. All of these works indicate that the supporting substrates (metal oxides (MOx)/nanoparticles (NPs)) have a synergistic effect on the properties of the intrinsic NPs, giving the composites a much greater potential for use in SERS applications compared to the NPs alone.16–18 The properties of MOx can be modified by incorporating metal NPs and thus obtaining a great enhancement in the SERS signals.19,20 Moreover, several studies have focused on fabricating flexible SERS substrates, in order to further develop their innovative use as bendable supports. Compared with conventional rigid substrates, flexible substrates endow opto-electronic devices with unique properties, such as flexibility, portability and/or disposability. Fox example, Pimentel et al.21 fabricated a ZnO nanorod decorated with Ag nanoparticles supported by a flexible cardboard platform. When using rhodamine 6G (R6G) as the test analyte, a Raman enhancement factor of 7 × 105 was obtained for this SERS substrate, and the distribution of “hot spots” on the substrate is generally believed to affect the SERS performance.22 Later, Oliveira et al.23 distributed Ag nanostars on a paper with high porosity, and this exhibited a better SERS performance than that of the paper with low porosity. More recently, a new substrate composed of Ag nanoflowers on a graphene@Cu net (AgNFs/G@Cu) was prepared by Zhang et al.,24 who obtained a flexible substrate for flexible SERS application. These works suggest that porous, flexible and conductive substrates show efficient SERS enhancement.

As a common metal oxide, MnO2 has been extensively investigated owing to its low cost, natural abundance, various morphologies, and low toxicity.25 These advantages provide it with a wide range of applications in catalysis, ion exchange, molecular adsorption, biosensors, and energy storage.26 MnO2 has various constructions including particles, rods, wires, tubes, sheets and 3D porous nanostructures, in which porous MnO2 frameworks are a significant research area owing to their superiority to bulk counterparts in many aspects, such as their higher surface area and the fact that they possess a lower dead volume.27 This provoked us to develop novel composite materials as highly SERS-active substrates.

Herein, we report a facile method to fabricate a flexible MnO2 porous construction on aluminum foil using a hydrothermal method, and subsequently decorate these porous flakes structures with Ag nanoparticles (AgNPs) achieved using a wet chemical method. Three kinds of MnO2@Al supports with different frameworks were obtained by controlling the hydrothermal reaction time of the Al foil in the KMnO4 solution. During the following investigation, we found that the loading amount of the AgNPs is dependent on the morphology and structure of the MnO2@Al substrate. By comparing the SERS performance of the three kinds of support, the AgNPs/MnO2@Al (18 h) sample was found to have the best properties for the detection of R6G. This is attributed to the 3D porous framework which offers more sites for aggregation of the Ag particles, giving the SERS signal enhancement. In addition, we found a new application for Al foil in this study, which could be helpful for further investigation of other metal foils.

2. Experimental section

2.1 Materials and substrates

Commercially available Al foil (99.9% purity) was obtained from Sino pharm Chemical Reagent Ltd. Co. All other reagents and solvents were purchased from Alfa Aesar and were analytical grade and used without further purification. High-purity Milli-Q water (18.2 MΩ) was used throughout the study.

2.2 Preparation of MnO2 nanosheets on Al foil

Aluminum foil (30 × 30 mm) was first immersed in the diluted hydrochloric acid solution to remove the oxide/hydroxide layer from the surface, and cleaned with acetone, alcohol and deionized water via ultrasonication for 10 min to remove the organic pollutants respectively. After drying with high purity N2, it was immersed in a solution containing KMnO4 (0.1 M, 30 mL). The aqueous solution and the Al foil were transferred to a Teflon-lined stainless-steel autoclave, which was maintained at 160 °C for 12, 18 and 24 h, respectively. Subsequently, the sample was washed with distilled water and ethanol, and dried at 60 °C overnight.

2.3 Preparation of AgNPs/MnO2@Al nanocomposites for SERS measurement

An AgNPs/MnO2@Al hybrid was synthesized via a wet chemical method. Briefly, silver sol was first prepared by dropping trisodium citrate (0.34 mM, 10 mL) into the silver nitrate solution (90 mg, 500 mL) which was boiling and being stirred. After cooling to room temperature, the obtained silver sol was aged for several days before use. During the heating process, the color of the mixture changed from colorless, to yellow, then orange and then finally a grayish yellow. Moreover, an obvious black precipitate was generated at the bottom of the beaker. At last, different MnO2@Al samples were immersed in the silver sol solution for 0.5 h and dried in air.

2.4 Characterization and SERS measurement

Powder X-ray diffraction (XRD, D/max 2500, Cu Kα) was used to identify the composition of the samples. The surface morphologies of the samples were observed using scanning electron microscopy (SEM) (ZEISS AURIGA FIB/SEM) with an energy dispersion X-ray spectrometer (EDS). Atomic force microscopy (AFM) (Nanonavi E-Sweep, SII, Japan) was also used in the tapping mode at room temperature in air. R6G solutions (2 μL) (Sigma-Aldrich) of different concentrations were dropped onto samples before the SERS measurement. The SERS spectra were acquired with a laser confocal Raman spectrometer (Horiba Jobin Yvon LabRAM HR Evolution) equipped with a 50× objective lens of numerical aperture (NA) 0.75, at a work distance (WD) of 0.37 mm, using an air cooled frequency doubled Nd:YAG green laser (λ = 633 nm, P = 50 mW with a 10% filter) at room temperature. An accumulation time of 2 s was used in the tests to avoid the heating effect generated by the laser.

3. Results and discussion

3.1 Synthesis and characterizations of AgNPs/MnO2@Al

Scheme 1 depicts the synthesis route for the AgNPs/MnO2@Al. During the process, the MnO2 nanoflakes were decorated onto the surface of the Al foil via a reaction with the KMnO4 solution under hydrothermal conditions. The reaction involved in the formation of the MnO2 nanosheets is expressed as follows:28
 
2KMnO4 + 2H2O → 2MnO2 + 2K+ + 4OH + O2 (1)

image file: c8ra07778a-s1.tif
Scheme 1 Schematic illustration of the synthesis process for the AgNPs/MnO2@Al array.

Impressively, the MnO2 sheets provide abundant immobilization sites for the silver nuclei, as well as a spacious template for the adhesion of the silver nanoparticles.

The silver colloid was prepared via the chemical reduction method and based on the research published by Lee and Meisel. During the process, silver nitrate serves as the silver precursor and trisodium citrate is the reductant.29 The reaction mechanism can be expressed as follows:30

 
4Ag+ + C6H5O7Na3 + 2H2O → 4Ag0 + C6H5O7H3 + 3Na+ + H+ + O2 (2)

The single crystalline characteristics of MnO2@Al and AgNPs/MnO2@Al were investigated using XRD, and the corresponding spectra are shown in Fig. 1. For these two samples, the diffraction peaks at about 12.5°, 36.2° and 42.5° from the MnO2 match the standard XRD pattern for a birnessite-type manganese oxide crystal (JCPDS 80-1098).31 Although the standard XRD pattern for Ag (JCPDS 04-0783)32 and Al (JCPDS 85-1327) are similar, a new peak for a (111) plane can be clearly observed for the AgNPs/MnO2@Al sample, but not for the MnO2@Al sample, suggesting the successfully fabrication of the AgNPs on the MnO2@Al substrate. In addition, some undefined peaks corresponding to the Al2O3 phase (JCPDS 70-3322) are due to the strong oxidation ability of KMnO4.


image file: c8ra07778a-f1.tif
Fig. 1 XRD pattern of MnO2@Al and AgNPs/MnO2@Al composite.

Fig. 2 presents typical SEM images and photos for the MnO2@Al products obtained at different reaction times. As shown in Fig. S1 (ESI), the surface of the original aluminum foil is smooth and shows a silver color in the inset of Fig. S1. After the aluminum foil reacts with the KMnO4 solution at 160 °C for different times, MnO2@Al samples with various porous frameworks consisting of MnO2 nanoflakes are clearly observed in Fig. 2a–c. Meanwhile, the color gradually changes from a brass color to black as seen in the insets of Fig. 2a–c. After 12 h under hydrothermal conditions, the net-like morphology of the MnO2 nanosheets was formed on the aluminum foil (Fig. 2a and d). When the reaction process was increased to 18 h, the porous structure was found to be larger than that after 12 h (Fig. 2b and e). However, the MnO2 nanoflakes tended to aggregate and became crossed with each other as the time was extended to 24 h (Fig. 2c and f), which would thus reduce the porous structure. In addition, Fig. S2 (ESI) shows a cross-section SEM image for the MnO2@Al prepared at 18 h, which also suggested that the net-like framework was made of flakes.


image file: c8ra07778a-f2.tif
Fig. 2 The SEM images of MnO2@Al prepared with different lengths of time: (a and d) 12 h; (b and e) 18 h; (c and f) 24 h, the inset is the digital image of the corresponding products.

The SEM images of the AgNPs/MnO2@Al samples are presented in Fig. 3. It was observed that the AgNPs were distributed on the top surface of the MnO2 nanoflakes when the MnO2@Al (12 h) acts as the support (Fig. 3a). However, except for the AgNPs scattered on the outside surface of the MnO2@Al (18 h) substrate, many of the silver particles embedded in the porous framework were made of larger MnO2 nanosheets (Fig. 3b). As the hydrothermal time was increased to 24 h, the AgNPs were found to be distributed on the surface of porous structure again, rather than embedded in the pores (Fig. 3c), which was due to the crossed over larger MnO2 sheets which narrow the holes. The element mapping images of the AgNPs/MnO2@Al sample (18 h) are shown in Fig. 3d. It can be seen that there is a highly homogeneous distribution of the O, Al and Mn in the sample, which is in line with the results from SEM obtained previously. With respect to the element distribution of Ag, the silver particles aggregated on the surface of the MnO2 flakes can be clearly observed, while those embedded in the porous framework are not included.


image file: c8ra07778a-f3.tif
Fig. 3 The SEM images of (a) AgNPs/MnO2@Al (12 h); (b) AgNPs/MnO2@Al (18 h); and (c) AgNPs/MnO2@Al (24 h). (d) The corresponding EDS mapping for AgNPs/MnO2@Al (18 h).

Atomic force microscopy is a highly precise technique that can provide topographical and compositional information on the surface of materials. Herein, AFM pictures of the MnO2@Al (18 h) substrates before and after the deposition of silver nanoparticles are shown in Fig. 4. The porous structure can be observed from the Fig. 4a and b, which is in accordance with results previously obtained using SEM. After the deposition of silver nanoparticles, the nanoparticles can clearly be seen from the AFM picture (the white dotted circles in Fig. 4c and d), confirming that the silver particles are embedded into the MnO2 flakes successfully. In addition, the AgNPs are randomly distributed on the surface and are prone to aggregation during the deposition process. Analysis of the AFM data (Fig. 4b and d) indicates that the AgNPs/MnO2@Al (18 h) show a greater nanoscale roughness (RMS = 14.75 nm) compared to the hierarchical MnO2@Al (18 h) architecture (RMS = 9.69 nm), which may be ascribed to more Ag NPs being embedded in the holes resulting in the reduction of pores.33,34


image file: c8ra07778a-f4.tif
Fig. 4 AFM images of MnO2@Al (18 h) before (a), (b) and after (c), (d) deposition of silver colloidal nanoparticles. The white dotted circles show the location of the AgNPs on the MnO2@Al substrate.

3.2 Raman spectrum

Fig. 5a shows the Raman spectra of the MnO2@Al and AgNPs/MnO2@Al samples. The AgNPs/MnO2@Al product shows two additional Raman peaks at about 854 and 1059 cm−1, the peak at 1059 cm−1 belongs to the aromatic C–H bending of the silver particles, while 854 cm−1 is not a typical peak and may be caused by complex coupling among MnO2, Al and Ag.35
image file: c8ra07778a-f5.tif
Fig. 5 (a) Raman spectra of MnO2@Al and AgNPs/MnO2@Al; and (b) SERS activity of Al foil, MnO2@Al, and the AgNPs/MnO2@Al composite for R6G.

3.3 SERS activity of Al foil, MnO2@Al and AgNPs/MnO2@Al

The SERS activities of these three samples were evaluated using the detection of R6G. Fig. 5b depicts the SERS spectra of R6G on the AgNPs/MnO2@Al composite (top curve), MnO2@Al (middle curve) and Al foil (bottom curve). There is no obvious SERS signal for the Al foil and MnO2@Al samples, but AgNPs/MnO2@Al shows a prominent improvement (at 613, 1181 and 1506 cm−1) for the detection of R6G. By comparison, it is clear that the role of the AgNPs in this configuration is the key to the detection of the R6G analyte.36 Moreover, the high density of AgNPs results from the large specific surface area and the porous structure of the immobilized MnO2 flakes can generate more hot spots and increase the loading of the analyte, which is beneficial to the SERS signal.9,37

In our previous report, the amount of AgNPs played an important role in the detection of R6G. In this work, it was also found that the amount of adhesion of the AgNPs was also strongly dependent on the structure and morphology of the substrate. We systematically investigated the influence on the detection of R6G through a series of experiments comparing the three kinds of MnO2@Al supports while keeping the other conditions unchanged. The SERS spectra for 10−3 M and 10−6 M of R6G molecules adsorbed onto the samples AgNPs/MnO2@Al (12 h), AgNPs/MnO2@Al (18 h) and AgNPs/MnO2@Al (24 h) are presented in Fig. 6a and b respectively. In a comparison to the SERS signals for the three substrates, the SERS intensity decreased in the sequence of AgNPs/MnO2@Al (18 h), AgNPs/MnO2@Al (12 h) and AgNPs/MnO2@Al (24 h). When using AgNPs/MnO2@Al (18 h), the SERS intensity of R6G increased almost four times for the 1361 cm−1 peak compared with the AgNPs/MnO2@Al (24 h) sample. The enhanced outcomes are due to the high density of the AgNPs and small “hot spots” on the SERS substrates, which causes a strong plasmonic coupling effect between the adjacent AgNPs,38 and where the electromagnetic field can be amplified dramatically.39 For the sample AgNPs/MnO2@Al (18 h), more AgNPs were adsorbed onto the porous framework made of MnO2 sheets, in other words, the gap between the two adjacent AgNPs decreases as the silver loading increases, which can be confirmed using the SEM images.


image file: c8ra07778a-f6.tif
Fig. 6 The SERS spectra of the R6G molecules collected from the AgNPs/MnO2@Al samples (12 h, 18 h, 24 h) at different concentrations of (a) 10−6 M and (b) 10−3 M.

To demonstrate the performance of our prepared AgNPs/MnO2@Al (18 h), the SERS sensitivity was investigated with different concentrations of the R6G solution ranging from 10−6 M to 10−3 M. As shown in Fig. 7a, the SERS detections were completed by altering the concentration of R6G. Clear peaks were observed in the three curves, and the vibration peaks at 1184, 1310, 1361, 1509, and 1647 cm−1 were assigned to the C–O–C stretching, C–H in-plane bending, and C–C stretching of the aromatic ring of the R6G molecule, respectively, while the peak at 770 cm−1 was derived from the hydrogen atoms of the xanthene skeleton and the out-of-plane bending motion.37,40,41 Fig. 7b shows the relationship between the SERS intensity of R6G and its concentration at 1361 cm−1 and 1509 cm−1, which is an exponential increase. The Raman signal is still observable when the molecule concentration is as low as 10−6 M (Fig. 7c), in which the relative intensities of 612 and 1509 cm−1 are about 50 and 40 counts, respectively, indicating the high sensitivity of our substrates. The excellent performance can be ascribed to the porous structure of the MnO2 sheets which provides more sites for aggregation of Ag particles.


image file: c8ra07778a-f7.tif
Fig. 7 (a) SERS spectra of R6G with six different molecular concentrations of AgNPs/MnO2@Al (18 h); (b) SERS intensity at 1361 cm−1 (squares) and 1509 cm−1 (circles) for different concentrations of R6G, the curves represent the fit to the experimental data; and (c) the SERS spectrum of R6G at 10−6 M.

4. Conclusions

In conclusion, we have used a facile hydrothermal and wet chemical method to construct flexible substrates based on incorporating AgNPs onto MnO2 nanoflakes supported on Al foil. The as-prepared AgNPs/MnO2@Al flexible sample was characterized in detail using instrumental techniques such as SEM, XRD and AFM. Owing to their porous, flexible and conductive features, a high sensitivity (10−6 M) was obtained when using the AgNPs/MnO2@Al as a SERS substrate for the detection of R6G. Moreover, the effect of the MnO2 morphology on the SERS performance were discussed. The experiment results suggest that the AgNFs/MnO2@Al substrates could be used for novel and practical SERS applications in the dyestuff industry.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

The authors gratefully acknowledge the financial support provided by the National Natural Science Foundation of China (Grant No. 21576034), the Innovative Research Team of Chongqing (CXTDG201602014), the State Education Ministry and Fundamental Research Funds for the Central Universities (106112017CDJQJ138802, and 106112017CDJSK04XK11) and the Graduate Research and Innovation Foundation of Chongqing, China (Grant No. CYB18002). The authors would like to thank Prof. Qian Chen at Chongqing University for language polishing. The authors also thank the Electron Microscopy Center of Chongqing University for material characterizations.

References

  1. T. Gao, Y. Wang, K. Wang, X. Zhang, J. Dui, G. Li, S. Lou and S. Zhou, ACS Appl. Mater. Interfaces, 2013, 5, 7308–7314 CrossRef CAS PubMed.
  2. Y. Wang, K. Lee and J. Irudayaraj, J. Phys. Chem. C, 2010, 114, 16122–16128 CrossRef CAS.
  3. B. Guven, N. Basaran-Akgul, E. Temur, U. Tamer and I. H. Boyaci, Analyst, 2011, 136, 740–748 RSC.
  4. X. X. Han, Y. Ozaki and B. Zhao, TrAC, Trends Anal. Chem., 2012, 38, 67–78 CrossRef CAS.
  5. Y. He, Y. Wang, X. Yang, S. Xie, R. Yuan and Y. Chai, ACS Appl. Mater. Interfaces, 2016, 8, 7683–7690 CrossRef CAS PubMed.
  6. L. Qiu, W. Wang, A. Zhang, N. Zhang, T. Lemma, H. Ge, J. J. Toppari, V. P. Hytönen and J. Wang, ACS Appl. Mater. Interfaces, 2016, 8, 24394–24403 CrossRef CAS PubMed.
  7. A. Musumeci, D. Gosztola, T. Schiller, N. M. Dimitrijevic, V. Mujica, D. Martin and T. Rajh, J. Am. Chem. Soc., 2009, 131, 6040–6041 CrossRef CAS PubMed.
  8. M. Fan, G. F. Andrade and A. G. Brolo, Anal. Chim. Acta, 2011, 693, 7–25 CrossRef CAS PubMed.
  9. J. Zhao, Z. Zhang, S. Yang, H. Zheng and Y. Li, J. Alloys Compd., 2013, 559, 87–91 CrossRef CAS.
  10. L. Yang, Z. Bao, Y. Wu and J. Liu, J. Raman Spectrosc., 2012, 43, 848–856 CrossRef CAS.
  11. M. Roca and A. J. Haes, J. Am. Chem. Soc., 2008, 130, 14273–14279 CrossRef CAS PubMed.
  12. X. Tu, Z. Li, J. Lu, Y. Zhang, G. Yin, W. Wang and D. He, RSC Adv., 2018, 8, 2887–2891 RSC.
  13. X. Li, H. Hu, D. Li, Z. Shen, Q. Xiong, S. Li and H. J. Fan, ACS Appl. Mater. Interfaces, 2012, 4, 2180–2185 CrossRef CAS PubMed.
  14. Y. Wang, W. Song, W. Ruan, J. Yang, B. Zhao and J. R. Lombardi, J. Phys. Chem. C, 2009, 113, 8065–8069 CrossRef CAS.
  15. G. S. Kumar, R. G. Shrestha, Q. Ji, J. P. Hill, K. Ariga, S. Acharya and L. K. Shrestha, Phys. Chem. Chem. Phys., 2018, 20, 18873–18878 RSC.
  16. T. Gong, J. Zhang, Y. Zhu, X. Wang, X. Zhang and J. Zhang, Carbon, 2016, 102, 245–254 CrossRef CAS.
  17. M. Pradhan, A. K. Sinha and T. Pal, Chemistry, 2014, 20, 9111–9119 CAS.
  18. J. Zhang, X. Zhang, S. Chen, T. Gong and Y. Zhu, Carbon, 2016, 100, 395–407 CrossRef CAS.
  19. Z. Jie, W. Xinyu, Z. Pengyue, Q. Jiamin and Z. Yong, Opt. Express, 2016, 24, 24551–24566 CrossRef CAS PubMed.
  20. M. Xu, H. Niu, J. Huang, J. Song, C. Mao, S. Zhang, C. Zhu and C. Chen, Appl. Surf. Sci., 2015, 351, 374–381 CrossRef CAS.
  21. A. Pimentel, A. Araújo, B. Coelho, D. Nunes, M. Oliveira, M. Mendes, H. Águas, R. Martins and E. Fortunato, Materials, 2017, 10, 1351 CrossRef.
  22. E. C. Le Ru, P. G. Etchegoin and M. Meyer, J. Chem. Phys., 2006, 125, 204701 CrossRef CAS PubMed.
  23. M. J. Oliveira, P. Quaresma, M. Peixoto de Almeida, A. Araujo, E. Pereira, E. Fortunato, R. Martins, R. Franco and H. Aguas, Sci. Rep., 2017, 7, 2480 CrossRef PubMed.
  24. W. Zhang, P. Man, M. Wang, Y. Shi, Y. Xu, Z. Li, C. Yang and B. Man, Carbon, 2018, 133, 300–305 CrossRef CAS.
  25. F. Li, H. Chen, X. Y. Liu, S. J. Zhu, J. Q. Jia, C. H. Xu, F. Dong, Z. Q. Wen and Y. X. Zhang, J. Mater. Chem. A, 2016, 4, 2096–2104 RSC.
  26. S. Jana, S. Pande, A. K. Sinha, S. Sarkar, M. Pradhan, M. Basu, S. Saha and T. Pal, J. Phys. Chem. C, 2009, 113, 1386–1392 CrossRef CAS.
  27. M. Huang, F. Li, F. Dong, Y. X. Zhang and L. L. Zhang, J. Mater. Chem. A, 2015, 3, 21380–21423 RSC.
  28. Y. Zhang, T. X. Zheng, Y. B. Hu, X. L. Guo, H. H. Peng, Y. X. Zhang, L. Feng and H. L. Zheng, J. Colloid Interface Sci., 2017, 490, 226–232 CrossRef CAS PubMed.
  29. P. C. Lee and D. Meisel, J. Phys. Chem., 1982, 86, 3391–3395 CrossRef CAS.
  30. A. Sileikaite, I. Prosycevas, J. Puiso, A. Juraitis and A. Guobiene, J. Mater. Sci., 2006, 12, 287–290 Search PubMed.
  31. J. Ma, S. Zhu, Q. Shan, S. Liu, Y. Zhang, F. Dong and H. Liu, Electrochim. Acta, 2015, 168, 97–103 CrossRef CAS.
  32. Z. Liu, Y. Wang, R. Deng, L. Yang, S. Yu, S. Xu and W. Xu, ACS Appl. Mater. Interfaces, 2016, 8, 14160–14168 CrossRef CAS PubMed.
  33. G. Macias, M. Alba, L. F. Marsal and A. Mihi, J. Mater. Chem. C, 2016, 4, 3970–3975 RSC.
  34. J. Sánchez, J. Fullea, C. Andrade, J. J. Gaitero and A. Porro, Corros. Sci., 2008, 50, 1820–1824 CrossRef.
  35. M. L. Zhang, X. Fan, H. W. Zhou, M. W. Shao, J. A. Zapien, N. B. Wong and S. T. Lee, J. Phys. Chem. C, 2014, 114, 1969–1975 CrossRef.
  36. J. Huang, D. Ma, F. Chen, D. Chen, M. Bai, K. Xu and Y. Zhao, ACS Appl. Mater. Interfaces, 2017, 9, 7436–7446 CrossRef CAS PubMed.
  37. Z. Li, S. Jiang, S. Xu, C. Zhang, H. Qiu, C. Li, Y. Sheng, Y. Huo, C. Yang and B. Man, Sens. Actuators, B, 2016, 230, 645–652 CrossRef CAS.
  38. N. J. Halas, S. Lal, W. S. Chang, S. Link and P. Nordlander, Chem. Rev., 2011, 111, 3913–3961 CrossRef CAS PubMed.
  39. Q. Fu, Z. Zhan, J. Dou, X. Zheng, R. Xu, M. Wu and Y. Lei, ACS Appl. Mater. Interfaces, 2015, 7, 13322–13328 CrossRef CAS PubMed.
  40. S. S. Gao, S. B. Shang, X. Y. Liu, Z. Li, Y. Q. Sheng, C. Zhang, C. Yang, H. W. Qiu, Y. Y. Huo and S. Z. Jiang, RSC Adv., 2016, 6, 81750–81756 RSC.
  41. Y. Q. Wang, S. Ma, Q. Q. Yang and X. J. Li, Appl. Surf. Sci., 2012, 258, 5881–5885 CrossRef CAS.

Footnote

Electronic supplementary information (ESI) available. See DOI: 10.1039/c8ra07778a

This journal is © The Royal Society of Chemistry 2018