Open Access Article
This Open Access Article is licensed under a Creative Commons Attribution-Non Commercial 3.0 Unported Licence

Natural iron ore as a novel substrate for the biosynthesis of bioactive-stable ZnO@CuO@iron ore NCs: a magnetically recyclable and reusable superior nanocatalyst for the degradation of organic dyes, reduction of Cr(VI) and adsorption of crude oil aromatic compounds, including PAHs

S. Mohammad Sajadi*ab, Kamal Koloa, Mohammad Piroueiab, Sarbast A. Mahmudcd, Jagar. A. Alia and Samir M. Hamadae
aScientific Research Center, Soran University, PO Box 624, Soran, KRG, Iraq. E-mail: smohammad.sajadi@gmail.com; Tel: +9647503714550 Tel: +9647503714551
bDepartment of Petroleum Geosciences, Faculty of Sciences, Soran University, PO Box 624, Soran, KRG, Iraq
cDepartment of Biology, Faculty of Sciences, Soran University, PO Box 624, Soran, KRG, Iraq
dDepartment of Pharmacy, Rwandz Private Technical Institute, Rawanduz, Soran, KRG, Iraq
eResearch Center, Cihan University, Erbil, Iraq

Received 16th July 2018 , Accepted 3rd October 2018

First published on 16th October 2018


Abstract

For the first time, stable ZnO@CuO@iron ore nanocomposites (NCs) were green synthesized using magnetic iron ore as a natural substrate through an eco-friendly, simple and cost-effective method. The biosynthesized nanocatalyst was characterized using the SEM, EDS, elemental mapping, point analysis, XRD, FT-IR, polarized microscopy and UV-vis analytical techniques. The XRD and SEM methods confirmed the excellent stability of the nanocatalyst, even for 6 months. Also, the antioxidant ability of the green-synthesized NCs using a DPPH method was assessed per gallic acid and in contrast with ascorbic acid. Furthermore, their antibacterial activities against the common pathogenic bacteria of Pseudomonas aureus, Staphylococcus aureus and Escherichia coli were evaluated at different concentrations compared to chloramphenicol as a positive control. Moreover, the superior catalytic activity of the ZnO@CuO@iron ore NCs was investigated during a series of reactions, including the adsorption of polycyclic aromatic hydrocarbons (PAHs) of heavy crude oil (HCO) obtained from the Shaikhan oil field, the destruction of some organic dyes at room temperature, including methylene blue (MB) and methyl orange (MO), thymol blue (TB), bromothymol blue (BTB), phenol red (Ph.R), methyl red (MR), solochrome black T (SBT) and eriochrome black T (EBT) and finally the reduction of Cr(VI) at ambient temperature using UV-vis spectroscopy. Finally, the magnetic NCs could be simply recovered and reused several times without considerable loss of catalytic activity.


Introduction

Nature shows excellent capability in the synthesis of nanomaterials, in which biological systems are ‘bio-laboratories’ that produce nanomaterials for use in biomimetic pathways. These pathways are green, energy saving, cost effective and biocompatible for the deposition of biological molecules on the surface of green NPs.1–3 The large surface of metal oxide nanoparticles shows a large number of active sites per unit area compared to the parent metal, which in turn, are strongly related to their various applications. Current synthetic methods of NPs restrict their use to some medicinal applications involving the accumulation of poisonous and dangerous materials on a nanoproduct surface.4–7 In recent years, natural supporting materials have attracted the attention of researchers for their capacity to prevent the agglomeration and over-stoichiometric use of metal reagents and also to increase the stability of produced nanostructures by altering their sensitivity to oxygen, water and other chemical entities.8,9

Plants are a valuable source of some compounds with reductive abilities, called antioxidants. In fact, the antioxidant activity of plants is attributed to the redox potential of phytochemicals to quench singlet and triplet oxygen, decompose peroxides or neutralize free radicals.10–12 The higher bioactivity of nanoparticles could also be attributed to the large surfaces of nanoparticles and preferential adsorption of the bioactive constituents from an extract onto the surface of the nanoparticles, both of which are strongly affected by the surface area, particle size and surface reactivity of the nanoparticles.13–19

The toxicity and carcinogenic characteristics of organic dyes represent a series of problematic challenges to human life, thus developing efficient treatment methods to ensure the removal of organic dye pollutants is an essential requirement. The large surface area of nanostructures enhances significantly their ability in the catalytic degradation of organic dyes. Among the nanostructures, the green-synthesized ones have increasingly become the subject of many studies, as they do not show the side effects and the difficulties involved in use of the previous methods. One aim of this research was to study the ability and the efficiency of green-synthesized ZnO@CuO@iron ore NCs in the destruction of a wide spectrum of harmful organic dyes.20–22

Cr(VI) is one of the most dangerous heavy metals in the environment, and due to its solubility in water, its removal has challenged many researchers in recent years. Up to now, most studies on the removal of Cr(VI) have been based on its conversion to Cr(III), which has low toxicity and is easily eliminated through the formation of insoluble hydroxides by adjusting the pH in aqueous media. Recently, other reaction processes have focused on the reduction of Cr(VI). Most of these methods have problems, such as the production of secondary wastes and toxic by-products.23,24 This study uses ZnO@CuO@iron ore NCs as a highly efficient nanocatalyst to aid the removal of hexavalent chromium.

Polycyclic aromatic hydrocarbon (PAH) compounds are lipophilic and highly soluble in organic solvents and include fused aromatic rings with various toxicities produced mainly via the incomplete combustion and pyrolysis of materials containing carbon and hydrogen, such as coal, oil, wood and petroleum products.25,26 Many reports have confirmed that aromatic compounds, especially PAHs, are toxic and environmentally persistent with carcinogenic, immune suppressant and mutagenic effects. The main sources of polyaromatic compounds are pyrogenic, petrogenic and biological processes, in which those produced from petrogenic sources are the most widespread pollutants due to the considerable transportation, storage and application of crude oil and its products.27,28 This research work investigates the catalytic ability of the NCs to adsorb aromatic hydrocarbons, including PAHs, from Shaikhan crude oil.

The Shaikhan block is a large oilfield discovered in Iraqi Kurdistan in the last decade. The field was explored and developed by Gulf Keystone Petroleum Limited, see ESI, Fig. 1.

Bryonia dioica from the family Cucurbitaceae is indigenous to many parts of Europe and West Asia and is well distinguished from the other Bryonia species by its black fruits and monoecious flowers.29,30 Among the significant phytochemical content of Bryonia are alkaloid bryonicine and antioxidant flavonoids, such as saponarin, vitexin, isovitexin, 5,7,4′-trihydroxy flavone 8-C-glucopyranoside, lutonarin, isoorientin; glycosides, and also triterpenoids, cucurbitacin L, 23,24-dihydrocucurbitacin B, 23,24-dihydrocucurbitacin D, arvenin IV and also lipids, which are of special importance.31,32 The rich phytochemical content of the plant reported in the literature and the ability of its extract to reduce metal ions has made it a strong candidate for the synthesis of ZnO@CuO@iron ore NCs in a green way and the evaluation of its stability, bioactivities and applications, ESI, Fig. 2.

This study for the first time employed both the Bryonia dioica root extract as an antioxidant bioreducing, stabilizing and capping source and natural iron ore as a novel green substrate to synthesize ZnO@CuO@iron ore NCs as a green nanocatalyst. In fact, this natural substrate increases the synergic effect, stabilizing factor and prevents the agglomeration of anchoring nanoparticles. Furthermore, the stability and bioactivity of the nanocatalyst, including antioxidant activity (in contrast to ascorbic acid's antioxidant ability) and antibacterial activity against common pathogenic bacteria of Pseudomonas aureus, Staphylococcus aureus and Escherichia coli, were investigated. Also, the catalytic activity and adsorption ability of bioactive NCs was monitored during the destruction process of a wide series of harmful organic dyes, adsorption of the aromatic contents of Shaikhan crude oil and reduction of Cr(VI) at ambient temperature.

Experimental

Reagents and methods

High-purity chemicals were purchased from Merck and Aldrich chemical companies. X-ray diffraction (XRD) measurements were carried out using a Philips powder diffractometer type PW 1373 goniometer with scanning rate of 2° min−1 in the 2θ range from 0° to 90°. UV-visible spectra for analysis were recorded on a double-beam spectrophotometer (Super Aquarius) to monitor the SPR signals of the nanoparticles. The morphology, particle dispersion and chemical composition of the prepared nanostructures were investigated by fast emission scanning electron microscopy (FE-SEM) (Quanta 450) equipped with EDS (energy dispersive X-ray spectroscopy). FT-IR spectra were recorded on a Nicolet 370 FT/IR spectrometer (Thermo Nicolet, USA) using pressed KBr pellets. The antibacterial activity of the green-synthesized ZnO@CuO@iron ore NCs was studied using the disc diffusion method via Muller–Hinton media and by using chloramphenicol as positive control. The Pseudomonas aureus, Staphylococcus aureus and Escherichia coli were obtained from the Department of Biology, Soran University in KRG, Iraq.

Plant materials

The root of Bryonia dioica plant was collected in summer 2017 in the Haji Umran alpine region (at an elevation of 1705 metres above sea level) in Iraqi Kurdistan and identified by the Department of Biology of Soran University in Arbil, KRG, Iraq, Fig. 2.

Preparation of the Bryonia dioica root extract

First, 30.0 g of dried root powder of the plant was boiled in 300 mL double distilled water for 45 min at 80 °C. The obtained extract was centrifuged at 7000 rpm and then filtered and used for further steps of the study.

Magnetic iron ore collection

The iron ore deposit was collected in the north west of Choman, Erbil governorate, Iraqi Kurdistan, Fig. 1. The sample was washed with hot water to remove possible impurities then dried and powdered to be used as a natural magnetic support during this study.
image file: c8ra06028b-f1.tif
Fig. 1 Iron ore: (a) hand specimen, (b) natural outcrop setting.

One-pot green synthesis of ZnO@CuO@iron ore NCs

In a 250 mL flask, 1 g dried powdered iron ore was mixed with 100 mL plant extract, then 50 mL 0.6% CuCl2·2H2O and 0.2% Zn(NO3)2 solutions were added dropwise, respectively, to the mixture in an alkaline media that was adjusted using 0.1 M Na2CO3 at pH 9 with stirring at 80 °C until the colour of the mixture changed and formation of the precipitation occurred. The precipitation was then separated and heated at 105 °C for 2 h for autooxidation and formation of the ZnO@CuO@iron ore NCs. The obtained precipitate of NCs was washed with cool distillate water, then dried and kept for identification and application processes. The stability of the green nanocatalyst was detected using XRD analysis for six months after its synthesis.

Antimicrobial activity

Pseudomonas aureus, Staphylococcus aureus and Escherichia coli bacterial strains were used to evaluate the antibacterial activity of samples through a disc diffusion method by the standard protocol.33 Briefly, the overnight bacterial cultures (100 μL) were introduced over Muller–Hinton agar plates with a sterile glass rod. The minimum inhibition concentration (MIC) was determined for each sample, see Table 1. Also, the positive and negative controls were chloramphenicol and the discs were prepared using sterile distilled water. Briefly, 100 μL of the NCs and chloramphenicol (under the same conditions) were loaded on to the provided discs (6 mm D) and allowed to dry before being placed on the agar. The plates were inoculated at 37 °C for 24 h after incubation. Finally, the diameter of the inhibition zones was measured and tabulated.
Table 1 Antibacterial activity of Bryonia dioica root extract and ZnO@CuO@iron ore NCs
Compounds P. aureus S. aureus E. coli
a C+; chloramphenicol disc diameter (positive control).
Plant extract 19 mm 16 mm 13 mm
ZnO@CuO@iron ore NCs (1%) 29 mm 33 mm 28 mm
ZnO@CuO@iron ore NCs (2%) 37 mm 45 mm 47 mm
aChloramphenicol 13 mm 8 mm 13 mm


Antioxidant activity using the DPPH radical scavenging method

The antioxidant potential of the green-fabricated NCs against 2,2-diphenyl-1-picrylhydrazyl (DPPH) was determined using the method described by Clarke et al.34 Briefly, a 1[thin space (1/6-em)]:[thin space (1/6-em)]1 ratio of test sample (NCs) and ascorbic acid (for comparison) at different concentrations were mixed with freshly prepared DPPH solution in a test tube and kept in the dark for 30 min, respectively. Absorbance at 517 nm was measured with a UV-vis spectrophotometer and compared to an ascorbic acid inhibition curve. Furthermore, gallic acid was used as a control for both samples. Each assay was carried out in triplicate. The percentage inhibition of the DPPH radical was calculated using the following equation:
Radical Scavenging Activity (RSA%) or Inhibition (In%) = [(AcAt)/Ac] × 100
where In is the DPPH inhibition (%), Ac is the absorbance of the control and At is the absorbance of the samples. The amounts of both the NCs and ascorbic acid required to decrease the absorbance of DPPH by 50% (IC50) were calculated graphically as the mean value ± standard deviation and the results compared.

Reduction of organic dyes by ZnO@CuO@iron ore NCs

First, 20 mL of 3 × 10−5 M aqueous solution of MO (in the case of MB, TB, BTB, Ph.R, MR, SBT and EBT solution, the concentrations were the same, respectively) was added to 5 mg of ZnO@CuO@iron ore NCs (in the case of MB, TB, BTB, Ph.R, MR, SBT and EBT solutions, the employed catalyst amount was 3, 1, 2, 3, 3, 7 and 10 mg, respectively, Table 2) at room temperature. Then, 20 mL of freshly prepared aqueous solution of NaBH4 (5.3 × 10−3) was added to the mixture with stirring at room temperature. The progress of the degradation reaction was monitored by recording the time-dependent UV-vis absorption spectra of the mixture. At the end of the reaction, the catalyst was simply separated from the reaction system by filtration and washed with ethanol and dried for the next cycle of the process, see ESI, Fig. 3.
Table 2 Reduction time of dyes using different amounts of ZnO@CuO@iron ore NCs
Entry Dye (M) NaBH4 (M) Catalysta (mg) Time (s)
a ZnO@CuO@iron ore NCs.b Not completed.c Org.D: organic dyes.d Diff.A: different amounts.
1 MO 5.3 × 10−3 3 2 minb
2 MO 5.3 × 10−3 5 26 s
3 MO 5.3 × 10−3 8 31 s
4 MO 5.3 × 10−3 10 55 s
5 MB 5.3 × 10−3 1 1 minb
6 MB 5.3 × 10−3 3 15 s
7 MB 5.3 × 10−3 5 28 s
8 MB 5.3 × 10−3 7 29 s
9 BTB 5.3 × 10−3 2 20 s
10 BTB 5.3 × 10−3 5 22 s
11 BTB 5.3 × 10−3 7 22 s
12 BTB 5.3 × 10−3 10 22 s
13 MR 5.3 × 10−3 2 27 s
14 MR 5.3 × 10−3 3 20 s
15 MR 5.3 × 10−3 4 26 s
16 EBT 5.3 × 10−3 2 2 minb
17 EBT 5.3 × 10−3 5 102 s
18 EBT 5.3 × 10−3 7 66 s
19 EBT 5.3 × 10−3 10 50 s
20 TB 5.3 × 10−3 1 12 s
21 TB 5.3 × 10−3 2 18 s
22 TB 5.3 × 10−3 3 18 s
23 Ph.R 5.3 × 10−3 1 18 s
24 Ph.R 5.3 × 10−3 2 16 s
25 Ph.R 5.3 × 10−3 3 10 s
26 Ph.R 5.3 × 10−3 5 10 s
27 SBT 5.3 × 10−3 3 41 s
28 SBT 5.3 × 10−3 5 34 s
29 SBT 5.3 × 10−3 7 25 s
30 SBT 5.3 × 10−3 10 25 s
31 Org.Dc Absent Diff.Ad No reaction
32 Org.D 5.3 × 10−3 Absent No reaction


Catalytic activity of the green-synthesized ZnO@CuO@iron ore NCs for the reduction of Cr(VI)

To study the catalytic ability of ZnO@CuO@iron ore NCs to reduce hexavalent chromium, the reduction of potassium dichromate (K2Cr2O7) by formic acid was used as a model system. Here, 5.0 mg of the ZnO@CuO@iron ore NCs was added to 25 mL of aqueous solution of 3.5 mM Cr(VI). Then, 1.0 mL formic acid solution (90%) was added to the mixture under constant stirring at 50 °C. The reaction progress with time was monitored using a UV-vis spectrophotometer. After the end of the reaction process, the catalyst was washed using distilled water and then dried to use in the next cycle of the reaction.

Catalytic ability of the green-synthesized ZnO@CuO@iron ore NCs for the adsorption of crude oil aromatics

The catalytic activity of green-synthesized NCs was monitored according to the details in ESI, Scheme 1. Briefly, 50 mL of the heavy crude oil sample was impregnated on 5 g silica gel (G*60) and mixed to 100 mL distilled water under reflux conditions at 80 °C for 30 min to remove the possible salts and inorganic interferences. After separation of the water phase, the oil sample was added to a mixture of methanol[thin space (1/6-em)]:[thin space (1/6-em)]diethyl ether[thin space (1/6-em)]:[thin space (1/6-em)]benzene (3[thin space (1/6-em)]:[thin space (1/6-em)]1[thin space (1/6-em)]:[thin space (1/6-em)]1) and then ultrasonicated at 60 °C to obtain the aromatics and PAHs. In the next step, the different amounts of the ZnO@CuO@iron ore NCs were added to 20 mL of the extracted aromatics and ultrasonicated at 60 °C to study the effect of the catalyst amount on the rate of the adsorption process, Table 2. Finally, the nanocatalyst was separated from the mixture and washed with n-hexane and absolute ethanol, then dried to use in the next cycle of the process. The catalytic adsorption process was monitored using UV-vis spectroscopy to study the efficiency of the catalyst to adsorb the aromatic compounds.

Results and discussion

Bryonia dioica root extract was used as antioxidant media to synthesize both ZnO and CuO NPs and for their immobilization on iron ore as a novel support containing different types of minerals for the one-pot biosynthesis of bioactive stable ZnO@CuO@iron ore NCs, Scheme 1. The green nanocatalyst was absolutely identified by various techniques, such as FE-SEM, EDS, XRD, FT-IR and UV-vis spectroscopy. Furthermore, the stability, bioactivity and catalytic ability of the prepared iron ore based nanocatalyst were studied.
image file: c8ra06028b-s1.tif
Scheme 1 Green-synthesis mechanism of ZnO NPs and CuO NPs using the antioxidant extract of the Bryonia dioica extract.

Characterization of Bryonia dioica extract

Fig. 2 shows the UV-vis signals of plant extract at 320 nm (bond I) and 267 nm (bond II) assigned to the cinnamoyl and benzoyl systems of antioxidant phenolics, respectively.35
image file: c8ra06028b-f2.tif
Fig. 2 UV-vis spectroscopy of Bryonia dioica root extract.

The signals around 3425, 1643, 1411 and 1300 to 1000 cm−1 correspond to the OH, carbonyl group (C[double bond, length as m-dash]O), stretching C[double bond, length as m-dash]C aromatic ring and C–O vibrations, respectively, Fig. 3. Therefore, the obtained results by FT-IR and UV-vis analysis support the reported results in previous literature, indicating the presence of phenolic antioxidants inside the plant extract.


image file: c8ra06028b-f3.tif
Fig. 3 FT-IR signals of the plant leaf extract.

Identification of natural iron ore substrate

From a geological point of view, the ore body was located at Choman in the Iraqi Zagros thrust zone (IZTZ), which belongs to the Alpine-Himalayan orogenic belt.

As Fig. 1 shows, the appearance of the iron ore hand sample is black coloured with high density, which contains large crystals of quartz. In fact, according to mineralogical studies of the ore body by polarized microscopy and X-ray diffraction (XRD) analysis, the ore is composed of quartz, magnetite, hematite, and chromite, Fig. 4.


image file: c8ra06028b-f4.tif
Fig. 4 Polarized microscopy image of iron ore sample; (a) and (b) show the microscopic pictures of ore body containing quartz (q) and opaque minerals (O).

Fig. 5 depicts the XRD analysis of the iron ore substrate. According to this diagram, the sample includes various mineral constituents, especially a suitable amount of magnetite, which supports the excellent magnetic properties of the iron ore sample. Also, from the XRD diagram of the sample, a homogenous crystalline structure involving magnetite, hematite, quartz and chromite constituents can be simply monitored.


image file: c8ra06028b-f5.tif
Fig. 5 XRD diagram of natural iron ore substrate.

For more convenience about the structural and constitutional elucidation of the natural iron ore sample, the surface morphology and elemental constituents of the sample were investigated with FE-SEM, EDS and elemental mapping, as depicted in Fig. 6–8. As concluded from the iron ore morphology, the SEM and EDS results show the presence of phases that are mainly enriched in Fe, Si, Cr, Al and Mg. Chromium, Al, Mg and some amount of Fe are concentrated in chromite minerals with a size of 20–120 micron, with the silica concentrated inside quartz grains as a single crystal with a size of 60 micron, and also in most areas as anhedral and fine grained and distributed unevenly inside the sample. Magnetite and hematite are the minerals of iron as a single grain (magnetite) and also in matrix (hematite).


image file: c8ra06028b-f6.tif
Fig. 6 SEM micrograph of natural iron ore substrate.

image file: c8ra06028b-f7.tif
Fig. 7 EDS micrograph of natural iron ore substrate.

image file: c8ra06028b-f8.tif
Fig. 8 Elemental mapping of the green-synthesized ZnO@CuO@iron ore NCs.

Green synthesis and characterization of the ZnO@CuO@iron ore NCs

The ZnO@CuO@iron ore NCs were synthesized using the natural based iron ore and Bryonia dioica extracts without the need for the application of toxic, hazardous or dangerous materials, such as surfactants and reductants. The crystallinity of the green-synthesized NCs is depicted in the XRD pattern in Fig. 9, which clearly shows the characteristic peaks of the crystal planes of various crystalline minerals, especially ZnO and CuO NPs.
image file: c8ra06028b-f9.tif
Fig. 9 XRD pattern of green-synthesized NCs.

The XRD signals of ZnO NPs at 31.841°, 34.507°, 36.324°, 47.592°, 56.634°, 62.895°, 66.426°, 67.983°, 69.091° and 72.987° show the (100), (002), (101), (102), (110), (103), (002), (112), (201) and (202) planes, respectively, which obviously show its crystalline monoclinic structure. Furthermore, Fig. 9 shows the crystalline nature of the CuO NPs. The XRD pattern indicates that the CuO nanoparticles had a face-centred cubic (fcc) structure. The CuO NPs had a similar diffraction profile observed to be at 32.47°, 35.49°, 38.68°, 48.85°, 53.36°, 58.25°, 61.45°, 68.45°, 72.31° and 75.48°, which were assigned to the (110), (111), (200), (202), (020), (202), (113), (311), (220) and (400) crystallographic planes of the face-centred cubic (fcc) crystals.

The FT-IR analysis of the nanocomposite strongly confirmed the deposition of phytochemicals on the surface of the nanostructure. The main peaks at 3387, 1643 and 1561 cm−1 are assigned to the functional groups of OH, C[double bond, length as m-dash]O and C[double bond, length as m-dash]C aromatic vibrations, respectively, Fig. 10. Therefore, the presence of bioactive phytochemicals on the surface of biosynthesized NCs, as depicted by the FT-IR spectrum, strongly justified the bioactivity of the green-synthesized NCs.


image file: c8ra06028b-f10.tif
Fig. 10 FT-IR spectrum of the green-synthesized nanocomposite.

In the next step, the preparation of the ZnO@CuO@iron ore NCs was further investigated by using SEM, EDS and mapping methods. The surface morphology and elemental structure of the biologically synthesized NCs were investigated with FE-SEM, EDS, point analysis and elemental mapping images, as depicted in Fig. 11–14, respectively. As Fig. 11 shows, a spherical and homogenous morphology of the nanoparticles deposited on the surface of iron ore with the range size mostly between 40 nm and 85 nm is visible.


image file: c8ra06028b-f11.tif
Fig. 11 FE-SEM micrograph of green-synthesized ZnO@CuO@iron ore NCs.

image file: c8ra06028b-f12.tif
Fig. 12 EDS spectrum of green-synthesized ZnO@CuO@iron ore.

image file: c8ra06028b-f13.tif
Fig. 13 Point analysis of green-synthesized ZnO@CuO@iron ore NCs.

image file: c8ra06028b-f14.tif
Fig. 14 Elemental mapping of the green-synthesized ZnO@CuO@iron ore NCs.

Furthermore, the EDS spectrum and elemental mapping images show the chemical composition of the nanocomposite and depict the well-defined peaks of the main elements of Fe, O, Zn, Si and Cu; thereby these results confirm the successful anchoring of the CuO and magnetite NPs on the iron ore substrate, Fig. 12 and 13. Therefore, the mentioned analysis well proved the fabrication of the ZnO@CuO@iron ore NCs. Moreover, the result obtained by point analysis of a special section of the sample strongly supported the elemental composition obtained by the EDS result, Fig. 14.

Evaluation of antimicrobial activity of the biosynthesized ZnO@CuO@iron ore NCs

The antibacterial activity of the green-synthesized NCs was studied against Pseudomonas aureus, Staphylococcus aureus and Escherichia coli pathogenic bacteria by a disk diffusion method. The concentration of NCs used for this study was 1% (10 mg mL−1) and 2% (20 mg mL−1), and the results were compared with chloramphenicol as a positive control. All other test conditions were the same. The diameter of the appeared discs per millimetre as a minimum protection zone was reported for each of the samples. According to the ESI, Fig. 4 and Table 1, the plant extract demonstrated less antibacterial activity against Pseudomonas aureus, Staphylococcus aureus and Escherichia coli bacteria than the green NCs, which probably refers to the large surface area of the NCs and the accumulation of bioactive phytochemicals on its surface, as demonstrated in the FT-IR spectrum of the NCs, Fig. 14. Although, the 1% concentration of NCs demonstrated a better antibacterial potential against the nominated bacteria, the 2% concentration of NCs showed a more considerable ability for the removal of pathogenic bacteria than the 1% concentration sample and chloramphenicol as the positive control under the same conditions, which possibly showed the increasing effect of the deposited plant phytochemicals on the surface of NCs with increasing the amount of catalyst. Therefore, the amount of phytochemicals adsorbed on NCs is an important factor concerning their antibacterial activity.

Evaluation of antioxidant activity of the biosynthesized ZnO@CuO@iron ore NCs

This method is based on the reduction of antioxidants with DPPH (2,2-diphenyl-1-picrylhydrazyl) at 517 nm to discolouring of DPPH radicals through pairing off its odd electron. The IC50 (efficient concentration value) parameter was used for reporting the obtained results. Following the study of the antioxidant activity using this method for both the green-synthesized ZnO@CuO@iron ore NCs and ascorbic acid against gallic acid as control, the IC50 values were calculated as 29.07 and 32.61 ppm for the green-synthesized nanocomposite and ascorbic acid, respectively. Furthermore, the radical scavenging activity of the nanocomposite in concentrations more than 300 ppm was clearly higher than that of ascorbic acid, in which this parameter is the highest at the maximum dose of 500 ppm (79%) at compared with ascorbic acid (65%) at the same concentration, see ESI, Fig. 5. The antioxidant ability of the green-synthesized nanocomposite demonstrated the deposition of a considerable amount of antioxidant phytochemicals on the surface of nanostructure, which caused an antioxidant ability around the ascorbic acid as a powerful antioxidant due to their ability to transfer a hydrogen atom or an electron.

Catalytic activity of the green-synthesized ZnO@CuO@iron ore NCs for the reduction of harmful organic dyes

The focus here is on the catalytic ability of the green-synthesized NCs for the reduction of organic dyes in the presence of NaBH4. The process benefits from the adsorption of NaBH4 onto the surface of catalyst and the formation of a metal hydride. In the next step, the organic dyes adsorb onto the surface of the catalyst and are then reduced. Finally, the reduced dyes desorb from the catalyst surface to create a free space for the reaction to continue, Scheme 2. According to Scheme 2, two possible mechanisms for the catalytic degradation of organic dyes are available: producing moieties with amine functional groups or releasing the N2 gas and producing the rest of the dye.12,36,37 Also, in order to evaluate the performance and optimum amount of the green ZnO@CuO@iron ore NCs in the catalytic reduction of organic dyes, different amounts of catalyst were studied and the results are summarized in Table 2.
image file: c8ra06028b-s2.tif
Scheme 2 Schematic of the possible mechanisms for the general reduction of organic dyes using green-synthesized NCs.

As reported in Table 2, the optimum amounts of the catalyst for the destruction of MO, MB, BTB, MR, EBT, TB, Ph.R and SBT were 5, 3, 2, 3, 10, 1, 3 and 7 mg respectively in the presence of NaBH4 and at ambient temperature. Further, the fastest possible degradation times of these organic dyes using the mentioned optimum amount of the catalyst were 26 s for MO, 15 s for MB, 20 s for BTB, 20 s for MR, 50 s for EBT, 12 s for TB, 10 s for Ph.R and 25 s for SBT as they were monitored spectrophotometrically by decreasing the maximum absorbance and removing the maxima while decolourizing the organic dyes, Fig. 15. Also, Table 2 reveals that there was no reaction in the absence of NaBH4 or catalyst even after passing 2 days. Thus, these are necessary parameters for the degradation process.


image file: c8ra06028b-f15.tif
Fig. 15 Catalytic degradation of organic dyes using green-synthesized ZnO@CuO@iron ore NCs in the presence of NaBH4 and at ambient temperature.

Catalytic activity of green-synthesized ZnO@CuO@iron ore NCs for the reduction of Cr(VI)

To further study the catalytic ability of green-synthesized NCs, the reduction of Cr6+ to Cr3+ was studied spectrophotometrically. The reduction of Cr6+ to Cr3+ in the presence of potassium dichromate (K2Cr2O7) and formic acid as a source of Cr(VI) compounds and reducing agent, respectively, was selected as a model reaction. The presence of formic acid is necessary for the process as there would be no reaction in its absence. The Cr2O72− had an absorption peak around 345 nm, which originated from the electron transfer between metal (Cr6+) and ligand (oxygen), Fig. 16. As shown in Fig. 16, after adding a specified amount of catalyst, the absorption peak at 350 nm gradually decreases and vanishes within 80 s together with the disappearance of the light-yellow colour of the reaction mixture at the end of the reaction.
image file: c8ra06028b-f16.tif
Fig. 16 Catalytic reduction of Cr6+ using green ZnO@CuO@iron ore NCs in the presence of K2Cr2O7 and HCO2H.

The possible mechanism follows the decomposition of the formic acid into H2 and CO2 using ZnO@CuO@iron ore NCs and then the reduction of chromium Cr2O72− by bubbling H2 gas, Scheme 3. The best result was obtained with 5 mg of the catalyst and 1.0 mL of formic acid at 60 °C (Table 3, entry 4).


image file: c8ra06028b-s3.tif
Scheme 3 Reduction mechanism of Cr(VI) to Cr(III) using green synthesized ZnO@CuO@iron ore NCs.
Table 3 Catalytic reduction of Cr6+ using ZnO@CuO@iron ore NCs at 60 °C
Entry Catalyst (mg) Time
a Reaction was not completed.
1 No catalyst 12 ha
2 Iron ore substrate 250 s
3 ZnO@CuO@iron ore NCs (2 mg) 135 s
4 ZnO@CuO@iron ore NCs (5 mg) 80 s
5 ZnO@CuO@iron ore NCs (7 mg) 80 s
6 ZnO@CuO@iron ore NCs (10 mg) 80 s


Catalytic ability of green-synthesized ZnO@CuO@iron ore NCs to adsorb the aromatic compounds of crude oil at room temperature

The ability of NCs was tested as an adsorbant of the aromatic compounds in crude oil at room temperature, in which various amounts of the catalyst were used to optimize the process. According to Table 4, the best result was obtained using 7 mg of the catalyst (entry 8). Also, it showed that the best result obtained by the application of the substrate (iron ore) as adsorbent solely (entry 3) was 25 min; the application of lesser amounts of the substrate led to insignificant adsorptions even after 45 min (entries 1 and 2) and amounts greater than 15 mg did not change the adsorption rate (entries 4 and 5). As previously mentioned, the best adsorption time (8 min) was obtained by using 7 mg of the green catalyst (entry 8), which indicated the efficiency of ZnO@CuO@iron ore NCs in this process. According to entry 6, Table 4, the application of 3 mg of catalyst showed no considerable adsorption signal even after 28 min. Finally as Table 4 shows, the time of the adsorption process decreased with increasing the amount of the catalyst.
Table 4 Catalytic adsorption of Shaikhan crude oil aromatics at room temperature
Entry Catalyst Crude oil aromatics (mL) Catalyst (mg) Time
a A few adsorbed.
1 Iron ore substrate 20 mL 5 45 mina
2 Iron ore substrate 20 mL 10 45 mina
3 Iron ore substrate 20 mL 15 25 min
4 Iron ore substrate 20 mL 20 25 min
5 Iron ore substrate 20 mL 25 25 min
6 ZnO@CuO@iron ore NCs 20 mL 3 28 mina
7 ZnO@CuO@iron ore NCs 20 mL 5 20 min
8 ZnO@CuO@iron ore NCs 20 mL 7 8 min
9 ZnO@CuO@iron ore NCs 20 mL 15 8 min


In Fig. 17, using an optimum amount of the catalyst (7 mg, Table 4, entry 8) for the process demonstrated a very good ability of the catalyst to adsorb the aromatics inside the sample crude oil of Shaikhan after 8 min, in which no aromatics were detected using a UV-vis technique after this time. This ability probably refers to the presence of a considerable amount of phytochemicals on the surface of NCs, which besides the enhancement of the synergistic effect of the catalyst and its surface activity, probably captured the aromatic compounds of the crude oil through the formation of chemical bonds on the surface of the nanocatalyst, thus removing them from the sample media.


image file: c8ra06028b-f17.tif
Fig. 17 Adsorption of crude oil aromatics, including PAHs, using ZnO@CuO@iron ore NCs (7 mg catalyst and 20 mL aromatic sample).

Reusability, recyclability and stability of the ZnO@CuO@iron ore NCs

In this section, the reusability and recyclability of the catalyst for the Cr6+ reduction process and for the adsorption of aromatics containing PAHs from the Shaikhan crude oil sample are studied. As shown in Fig. 18, the nanocatalyst could be reused for the aromatics removal process at least 8 times with insignificant reduction of its adsorption ability.
image file: c8ra06028b-f18.tif
Fig. 18 UV-vis spectroscopic detection of ZnO@CuO@iron ore NCs reusability to adsorb the crude oil aromatic compounds; (a) extracted aromatics, (b) adsorption process after 8 times of reusing the catalyst.

After ending the reaction process, the catalyst was easily separated from the reaction media by filtration and washing with n-hexane and finally dried at room temperature. Fig. 19 shows the SEM micrograph of the separated catalyst after the 8th cycle of the reaction. The SEM micrograph and its comparison to Fig. 11 show no significant changes in its morphology, shape and size, which indicates the high stability and efficiency of the green-synthesized NCs.


image file: c8ra06028b-f19.tif
Fig. 19 SEM micrograph of green-synthesized NCs after 8 times use in the aromatic removal process.

Furthermore, after 7 times use in the Cr6+-reduction process, the recyclability of the catalyst in this process was investigated by SEM micrograph. After each cycle of the reaction, the catalyst was easily separated and recovered conveniently by filtration from the reaction mixture, washing with hot methanol and finally dried to use in the next cycle of the process. The SEM analysis confirmed the excellent recyclability of the catalyst after the 7th run of the reaction, in which the surface morphology, shape and size of particles did not show any deviation from its normal position, as shown in Fig. 11. Therefore, it seems that the green-synthesized nanocatalyst showed constant characteristic and high recyclability in the Cr6+-reduction process, Fig. 20.


image file: c8ra06028b-f20.tif
Fig. 20 XRD pattern of the ZnO@CuO@iron ore NCs in the Cr6+-reduction process after 7 times being recycled.

For further investigation of the properties of the green-synthesized NCs, they were monitored after 6 months from their green synthesis. Fig. 21 depicts the XRD pattern of the green-synthesized NCs after 6 months, which in comparison to Fig. 13 simply demonstrated no significant difference with their normal position at the time of their synthesis, strongly confirming the high stability of the catalyst. It is understood here that the use of natural iron ore as a resistant substrate of the NCs and the presence of potent phytochemicals, including plant antioxidants, adsorbed on the surface of the NCs during their synthesis are the main factors that protect the catalyst from any decomposition and deformation processes and help maintain its morphology as stable and constant.


image file: c8ra06028b-f21.tif
Fig. 21 XRD pattern of the ZnO@CuO@iron ore NCs after 6 months from their green synthesis.

Conclusions

For the first time, a green, novel and economic strategy was employed to biosynthesize ZnO@CuO@iron ore NCs using the antioxidant content of Bryonia dioica extract and natural iron ore substrate. The synthesized NCs were well identified using XRD, SEM, EDS, elemental mapping, point analysis and FT-IR analytical techniques. The FT-IR spectrum of the NCs demonstrated the deposition of bioactive phytochemicals on the surface of the catalyst. Investigations of the antimicrobial and antioxidant potential of the green-synthesized nanocatalyst demonstrated its strong bioactivity compared to the related controls. The nanocatalyst was employed to remove crude oil aromatics, including PAHs, under mild conditions and demonstrated a high level of adsorption as monitored by UV-vis spectroscopy. Furthermore, its superior catalytic ability was monitored in the degradation process of a series of harmful organic dyes, such as MO, MB, TB, BTB, Ph.R, MR, SBT and EBT, and also in the reduction of hexavalent chromium (Cr6+) at room temperature, with its good potential and efficiency in both reactions demonstrated. Moreover, the reusability and recyclability of the green catalyst for aromatics removal and the reduction of hexavalent chromium was detected using UV-vis and SEM analysis, in which its high potential was confirmed for both reactions even after the 8th and 7th cycle of the process without losing its catalytic activity, respectively. Finally, the excellent stability of the biosynthesized ZnO@CuO@iron ore NCs was detected using XRD pattern after 6 months since their green synthesis.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

The authors gratefully acknowledge the lab facilities and technical support offered by the Scientific Research Center in Soran University to carry out this work.

References

  1. M. A. Albrecht, C. W. Evans and C. L. Raston, Green Chem., 2006, 8, 417 RSC.
  2. P. Dauthal and M. Mukhopadhyay, Ind. Eng. Chem. Res., 2016, 55, 9557 CrossRef CAS.
  3. K. B. Narayanan and N. Sakthivel, Adv. Colloid Interface Sci., 2010, 156, 1 CrossRef CAS PubMed.
  4. M. Hosseinkhani, M. Montazer, S. Eskandarnejad and M. K. Rahimi, Colloids Surf., A, 2012, 415, 431 CrossRef CAS.
  5. H. Meftahizade, J. Med. Plants Res., 2011, 17, 4310 Search PubMed.
  6. G. Schmid, Chem. Rev., 1992, 92, 1709 CrossRef CAS.
  7. F. Li, B. Zhang, S. Dong and E. Wang, Electrochim. Acta, 1997, 42, 2563 CrossRef CAS.
  8. W. Kim, J. Park, Y. Jang, Y. Chung, S. Hwang and T. Hyeon, Nano Lett., 2003, 3, 1289 CrossRef.
  9. A. Nemamcha and J. Rehspringer, J. Phys. Chem. B, 2006, 110, 383 CrossRef CAS PubMed.
  10. Z. Wei, C. Xu and B. Li, Bioresour. Technol., 2009, 100, 2883 CrossRef CAS PubMed.
  11. S. Xuan, Y. X. J. Wang, J. C. Yu and K. C. F. Leung, Langmuir, 2009, 25, 11835 CrossRef CAS PubMed.
  12. M. Nasrollahzadeh, S. M. Sajadic and A. Hatamifard, Appl. Catal., B, 2016, 191, 209 CrossRef CAS.
  13. A. R. Phull, Q. Abbas, A. Ali, H. Raza, S. J. kim, M. Zia and I. ul Haq, Future Journal of Pharmaceutical Sciences, 2016, 2, 31 CrossRef.
  14. W. Zhang and S. Y. Wang, J. Agric. Food Chem., 2001, 49, 5165 CrossRef.
  15. M. Atarod, M. Nasrollahzadeh and S. M. Sajadi, RSC Adv., 2005, 5, 91532 RSC.
  16. P. C. H. Hollman and I. C. W. Arts, J. Sci. Food Agric., 2000, 80, 1081 CrossRef CAS.
  17. M. G. Lindley, Trends Food Sci. Technol., 1998, 9, 336 CrossRef CAS.
  18. L. B. Colbert and E. A. Decker, J. Food Sci., 1991, 56, 1248 CrossRef CAS.
  19. M. Antolovich, P. D. Prenzler, E. Patsalides, S. McDonald and K. Robards, Analyst, 2002, 127, 183 RSC.
  20. M. Atarod, M. Nasrollahzadeh and S. M. Sajadi, J. Colloid Interface Sci., 2016, 462, 272 CrossRef CAS PubMed.
  21. M. Nasrollahzadeh, S. M. Sajadi and M. Khalaj, RSC Adv., 2014, 4, 47313 RSC.
  22. Z. Issaabadi, M. Nasrollahzadeh and S. M. Sajadi, J. Cleaner Prod., 2017, 142, 3584 CrossRef CAS.
  23. J. P. Metters, R. O. Kadara and C. E. Banks, Analyst, 2012, 137, 896–902 RSC.
  24. C. E. Barrera-Díaz, V. Lugo-Lugo and B. Bilyeu, J. Hazard. Mater., 2012, 223, 1 CrossRef PubMed.
  25. H. I. Abdel-Shafy and M. S. M. Mansour, Egypt. J. Pet., 2016, 25, 107 CrossRef.
  26. J. He, J. J. Li, Y. Wen, H. W. Tai, Y. Yu, W. C. Qin, L. M. Su and Y. H. Zhao, Chemosphere, 2015, 128, 111 CrossRef CAS PubMed.
  27. N. D. Dat and M. B. Chang, Sci. Total Environ., 2017, 609, 682 CrossRef CAS PubMed.
  28. O. E. Orisakwe, Z. N. Igweze, K. O. Okolo and N. A. Udowelle, Toxicol. Rep., 2015, 2, 1019 CrossRef CAS PubMed.
  29. B. M. Yashwanth, S. Shanker Rai and K. P. Shivalinge Gowda, World J. Pharm. Pharm. Sci., 2014, 4, 1120 Search PubMed.
  30. C. Montoliu, S. Valles, J. Renau Piqueras and C. Guerri, J. Neurochem., 1994, 63, 1855 CrossRef CAS PubMed.
  31. A. G. Panosyan, G. M. Avetissian, V. A. Mnattsakanian, S. G. Batrakov, S. A. Vartanian, E. S. Gabrielian and E. A. Amroyan, Planta Med., 1983, 47, 17 CrossRef CAS PubMed.
  32. L. M. Gogilashvili and E. P. Kemertelidze, Chem. Nat. Compd., 2000, 36, 399 CrossRef CAS.
  33. H. R. Madan, S. C. Sharma, D. Suresh, Y. S. Vidya, H. Nagabhushana, H. Rajanaik, K. S. Anantharaju, S. C. Prashantha and P. S. Maiya, Spectrochim. Acta, Part A, 2016, 152, 404 CrossRef CAS PubMed.
  34. G. Clarke, K. N. Ting, C. Wiart and J. Fry, Antioxidants, 2013, 2, 1 CrossRef CAS PubMed.
  35. S. V. Bhat, B. A. Nagasampagi and M. Sivakumar, Chemistry of Natural Products, Narosa Publishing House, New Delhi, 2005, p. 585 Search PubMed.
  36. L. Han, S. Xue, S. Zhao, J. Yan, L. Qian and M. Chen, PLoS One, 2015, 10, 1 Search PubMed.
  37. K. Naseem, Z. H. Farooqi, R. Begum and A. Irfan, J. Cleaner Prod., 2018, 187, 296 CrossRef CAS.

Footnote

Electronic supplementary information (ESI) available. See DOI: 10.1039/c8ra06028b