This work reports the photophysical properties of 1-thioglycerol capped hydrophilic terbium cation incorporated (doped) zinc sulfide [Zn(Tb)S] nanoparticles, which have been post-synthetically modified using Pb2+ [Zn(Tb)S/Pb] under ambient conditions with [Zn(Tb)S]
:
[Pb2+] = 1
:
10−5–1
:
10, essentially providing a scenario with low to heavy co-doping and ultimately the possibility of forming a material of different chemical identity. The effects of selected concentrations of [Zn(Tb)S]
:
[Mn+] = 1
:
1 and 1
:
10−2 have also been evaluated for the post-synthetic addition of Hg2+, Cd2+, Ca2+, Mg2+, Na+ and K+. The broad zinc sulfide nanoparticle and sharp Tb3+ emission have different dependence on the relative reactant concentration, with cation identity playing a significant role. The underlying photophysical processes have been rationalized based on the interplay among the (i) cation exchange, (ii) modification of the structural properties of the nanoparticles without necessarily exchanging the cations and (iii) emission enhancement of terbium dopants. In cases where Tb3+ emission is apparent, all the nanoparticles studied demonstrate an optical antenna effect, thus accessing a lower Tb3+ concentration regime compared to in bulk environments. The results presented provide an avenue for the detection of heavy metal ions in general and Pb2+ in particular, with a limit of detection that is at least in the range of sub-ppm, using either the broad ZnS or sharp Tb3+ emission, respectively. This strategy provides an avenue to combine (i) the extremely sensitive and easily accessible analytical technique of photoluminescence spectroscopy, (ii) post-synthetic modification reactions in semiconductor nanoparticles that can be performed with less experimental demand, (iii) time-gated measurement related to the longer luminescence lifetime of terbium cations and (iv) the simultaneous use of broad ZnS nanoparticle and sharp Tb3+ emission from the same assembly, helping eliminate false positive results.
Besides the occurrence of cation exchange reactions in the post-synthetic modification of appropriate semiconductor nanoparticles, other processes may also accompany this sort of chemical manipulation. For example, Murphy and co-workers have shown different photophysical properties in synthetically Mn doped Zn(Mn)S nanoparticles and the corresponding post-synthetically modified undoped ZnS nanoparticles.15 Chrysochoos and co-workers demonstrated modification of the surface properties of CdS nanoparticles when Cu2+ was added post-synthetically.16 Norris and co-workers studied CdSe nanoparticles with post-synthetic modification using Al3+, In3+ and Ag+ and discussed that the outcome of this chemical tuning depends on the dopant identity.17–19 Moreover, these authors demonstrated a change in n- to p-type doping with low and high Ag+ dopant amounts, and this was correlated to the dopant site being interstitial and substitutional, respectively. Towards a similar end, with regard to the post-synthetic modification of semiconductor nanoparticles, we previously demonstrated the operation of an optical antenna effect in sensitizing Tb3+ and Eu3+ photoluminescence when corresponding nitrate salts were added to a dispersion of ZnS nanoparticles in chloroform.20 Based on the hypothesis of surface sites being less symmetric compared to core sites, a comparison of the Eu3+ asymmetry ratio, luminescence lifetime and lifetime distribution indicates an enhanced surface related contribution in the post-synthetically treated nanoparticles compared to the corresponding synthetically incorporated counterparts. In summary, the post-synthetic modification of semiconductor nanoparticles opens up the possibility of cation exchange, or in cases where such exchange of cations is not feasible, the process may simply tune the surface properties of the nanoparticles, or the externally added cation may reside in the interstitial position of the nanoparticles, thereby tuning the properties of the nanoparticles. However, a systematic investigation of the photophysical properties of post-synthetically modified semiconductor nanoparticles as a function of the relative concentration of reactants is not evident in the literature. Investigating such reactant concentration dependent emission properties in semiconductor nanoparticles is the primary objective of the present study, with the cation identity playing a role in the underlying processes.
This study is organized as follows. Initially, Zn(Tb)S nanoparticles of a fixed concentration were treated post-synthetically with various concentrations of Pb2+ to assess the feasibility of a cation exchange reaction of Zn2+
:
Pb2+ and Tb3+
:
Pb2+ pairs in the investigated nanoparticles. This is followed by similar experiments using selected relative reactant concentrations of various other cations (Hg2+, Cd2+, Ca2+, Mg2+, Na+, and K+). Finally, the usefulness of combining post-synthetic modification of semiconductor nanoparticles and photoluminescence spectroscopy has been evaluated for the detection of heavy metal ions in general and Pb2+ in particular.
:
[Pb2+] was varied from 1
:
10−5 to 1
:
10. For the precipitation of the post-synthetically modified nanoparticles, acetone was added to the dispersion and this was centrifuged for 15 minutes at 3000 rpm. A similar procedure was adopted for the corresponding reactions with Mn+ (Hg2+, Cd2+, Ca2+, Mg2+, Na+ and K+), with 1
:
1 and 1
:
10−2 nominal concentrations of Zn(Tb)S and Mn+, respectively, to generate the Zn(Tb)S/M nanoparticles. To perform the reverse post-synthetic modification from the sample with [Zn(Tb)S]
:
[Pb2+] = 1
:
1, 10 times the amount of Zn2+ precursor that was initially used to make the Zn(Tb)S nanoparticles was added and the Tb3+ content was maintained at a 10% doping content.
The relative quantum yields (Φx) of the broad ZnS nanoparticle emission and sharp Tb3+ emission were calculated separately by comparison to the quantum yield of coumarin 153 (C153) dissolved in methanol (Φr = 0.42 (ref. 24)) using eqn (1),
![]() | (1) |
) is the luminescence intensity as a function of wavenumber
. The Tb3+ emission was extracted from the experimentally observed Zn(Tb)S nanoparticles emission spectrum by interpolating a baseline that corroborates with the ZnS nanoparticles emission only. For example, to obtain the Tb3+ emission band centered around 545 nm, first the experimentally observed emission spectrum of the Zn(Tb)S nanoparticles was interpolated with two data points in the wavelength range 520–570 nm, and this was further interpolated with data points having 1 nm data intervals, the same as that which was used for the experimental spectrum acquisition. A similar protocol was adopted to extract the other Tb3+ emission bands centered at 490, 585 and 620 nm. This interpolated background contribution was subsequently subtracted from the experimentally observed emission spectrum of the Zn(Tb)S nanoparticles to extract the separate contribution of the broad and sharp ZnS nanoparticles and Tb3+ emission, respectively.
The corresponding electronic absorption spectra are shown in panels e–h of Fig. 1. The Zn(Tb)S nanoparticles show characteristic absorption in the ultraviolet spectral range, which is consistent with higher band gap values. On increasing the concentration of Pb2+, the absorption contribution in the visible spectral region increases. In the sample with [Zn(Tb)S]
:
[Pb2+] = 1
:
10, the signature in the ultraviolet spectral range changes dramatically and concomitantly the contribution from visible absorption increases. This gradual change in the electronic absorption behavior of the samples is reflected in their color and can be perceived visually.
:
[Pb2+] = 1
:
1 show major bands at 2θ = 25.3°, 30.3°, 43.0°, 50.9°, 53.4°, 62.5°, 68.5° and 70.9° corresponding to the (111), (200), (220), (311), (222), (400), (331) and (420) planes of cubic lead sulfide [JCPDS card number: 05-0592] strongly indicating that addition of Pb2+ to the Zn(Tb)S nanoparticles leads to cation exchange of Zn2+ with Pb2+. It is worth noting that some bands at 2θ = 34.1°, 56.4° and 59.1° were left unassigned by us, and through a process of comparison of all the XRD peaks of terbium sulfide, we concluded that these bands are of non-noticeable contributions.
![]() | ||
Fig. 2 XRD profiles of the Zn(Tb)S nanoparticles and the sample with [Zn(Tb)S] : [Pb2+] = 1 : 1 are shown. | ||
:
[Pb2+] = 1
:
1 are presented in panels a and e of Fig. 3. The corresponding size distributions are shown in panels b and f. Collectively, these show the formation of particles that are spherical in shape with average diameters of 3.0 ± 0.5 nm and 3.9 ± 0.6 nm, respectively, before and after Pb2+ treatment. This suggests that the post-synthetic modification of the Zn(Tb)S nanoparticles with the given composition results in particles with a marginally increased size. The high resolution transmission electron microscopy (HRTEM) images shown in panels c and g of Fig. 3 identify different inter-planar distances that are correlated with the (111) and (200) planes of ZnS and PbS, respectively [JCPDS card numbers: 05-0566 and 05-0592 for ZnS and PbS, respectively]. Further support of this comes from the selected area electron diffraction (SAED) patterns, shown in panels d and h, identifying the different planes of ZnS and PbS, respectively. These measurements clearly identify the formation of a material of different chemical identity via the post-synthetic modification of the Zn(Tb)S nanoparticles with Pb2+.
The data presented in Fig. 3, while identifying the particle morphology with crystal information for the two extremes, does not directly shed light on the behaviour of the intermediate samples that have been prepared with various amounts of post-synthetically added Pb2+. To address this, corresponding electron microscopy experiments were undertaken with the samples having [Zn(Tb)S]
:
[Pb2+] = 1
:
10−4 and [Zn(Tb)S]
:
[Pb2+] = 1
:
10−2, and the data are shown in Fig. 4. For these two samples, particle diameters of 3.0 ± 0.5 and 3.2 ± 0.4, respectively, were observed. Moreover, the HRTEM and SAED patterns of these samples only reveal characteristic crystal planes that could be correlated with cubic zinc sulfide. This suggests that within the detection capability of the electron microscopy measurements performed in the present work, the formation of lead sulfide is not apparent using these reactant concentration ratios and Pb2+ is present as a dopant entity in the Zn(Tb)S nanoparticles. However, to this end, we note that elemental mapping would better address any specific and minor alterations in the Zn(Tb)S crystal during the post-synthetic modification of the nanoparticles. In general, elemental mapping of lanthanide incorporated semiconductor nanoparticles would reveal more detailed structural information with regard to the dopant spatial location in the semiconductor nanoparticles, however, the smaller dimension of the materials studied (∼3 nm in diameter) has restricted our efforts so far in obtaining elemental mapping using the available TEM facilities.
To summarize, both the Zn(Tb)S and PbS nanoparticles that have been prepared using [Zn(Tb)S]
:
[Pb2+] = 1
:
1 form cubic phases. The lattice parameters for the ZnS cubic phase are a = b = c = 5.406 Å, α = β = γ = 90° and for the PbS cubic phase the corresponding values are a = b = c = 5.936 Å, α = β = γ = 90°. These values indicate an increase in the volume of the nanoparticles upon transformation via cation exchange. As shown in Fig. 3, the diameter of the nanoparticles increases marginally following the post-synthetic modification of the Zn(Tb)S nanoparticles. This observation is in corroboration with the expected trend based on the crystal parameters.
:
[Pb2+] = 1
:
1 leads to a disappearance and marginal presence of the Zn and Tb bands, respectively, in the EDS, with a concomitant appearance of a Pb signature (panel b). This suggests that the cation exchange reaction of the Zn2+
:
Pb2+ pair is more facile compared to that of the Tb3+
:
Pb2+ pair. In the case where [Pb2+] has been further increased to [Zn(Tb)S]
:
[Pb2+] = 1
:
10, the complete disappearance of the Tb band occurs as well, with the signature of Pb being the sole cationic ingredient in the nanoparticles. This, along with the presence of an S band in the EDS, suggests the cation exchange of both Zn2+ and Tb3+ with the post-synthetically added Pb2+ and the formation of PbS nanoparticles with this relative concentration ratio. Many previous reports on cation exchange reactions have used a stoichiometric excess of the incoming cation compared to the outgoing cation in order to make the cation exchange reaction in semiconductor nanoparticles reach completion.4,25,26 This can be visualized with the concept of a limiting reagent. The relative concentrations of [Zn(Tb)S]
:
[Pb2+] = 1
:
10−5–1
:
10 cover scenarios ranging from a low to heavy amount co-doping and ultimately the formation of a material of different chemical identity. In this kind of reaction, any change in charge mismatch in the cationic components could be observed through the formation of appropriate defects and role of the surface capping ligands of the nanoparticles. On the other hand, any deviation in the size of the cations might be associated with a lattice distortion, as has been discussed by Banin and co-workers13 for doping Cu2+, Ag+ and Au3+ in InAs nanoparticles and by Chen and co-workers27 for doping Eu3+ in TiO2 nanoparticles. In the following section, the impact of post-synthetic modification of Zn(Tb)S nanoparticles as a function of [Pb2+] has been studied using photoluminescence spectroscopy (vide infra).
:
[Pb2+] = 1
:
1, following which a change in the spectral properties would be visible due to the formation of PbS nanoparticles via cation exchange. However, the experimentally observed trend has been found to have additional contributions that deviate from the spectral outcome predicted with this simplistic expectation. The following text first presents the data from photoluminescence spectroscopy measurements, and the roles of various processes in determining the spectral outcome are discussed.
The photoluminescence excitation and emission spectra of the Zn(Tb)S nanoparticles with post-synthetic modifications, through adding Pb2+ solutions with various [Pb2+], are presented in Fig. 6. Exciting the nanoparticles at 280 nm, the Zn(Tb)S nanoparticles reveal a characteristic broad emission band at 400 nm that is intrinsic to ZnS based materials and has been correlated to sulfur related vacancies.15,28–30 Additionally, the Zn(Tb)S nanoparticles show characteristic sharp emissions of Tb3+ at 490, 545, 585 and 620 nm that arise from the 5D4 → 7Fn [n = 6–3] transitions, respectively. These observations are consistent with our previous studies.20,22,30–32 The broad and sharp emissions of ZnS and Tb3+, respectively, in the Zn(Tb)S nanoparticles behave almost independently. It is worth noting that there exists million-fold differences between the radiative rates of the nanoparticles and Tb3+ intrinsic population decay kinetics. While the photoluminescence lifetimes of the ZnS nanoparticles are in the range of nanoseconds, these are in the order of milliseconds for the Tb3+ emission.
In the case where the Zn(Tb)S nanoparticles have been treated post-synthetically with Pb2+ of various concentrations, a non-monotonous trend has been observed in the emission behavior. A comparative summary of the relative intensities of the broad ZnS based nanoparticles emission centered at 400 nm and sharp Tb3+ emission as a function of [Pb2+] is presented in Fig. 7. The broad ZnS nanoparticles based emission decreases dramatically in the post-synthetically modified nanoparticles with [Zn(Tb)S]
:
[Pb2+] = 1
:
1 and 1
:
10, with respect to the corresponding intensity in the Zn(Tb)S nanoparticles. The [Zn(Tb)S]
:
[Pb2+] < 1
:
1 could be categorized differently. In the cases with [Zn(Tb)S]
:
[Pb2+] = 1
:
10−1–1
:
10−3 the broad emission is significantly lowered. It is noticeable that even when this ratio is 1
:
10−4, the emission decreases by a distinguishable extent. On the other hand, with this ratio being 1
:
10−5 this emission is comparable in magnitude to that observed in the Zn(Tb)S nanoparticles. Similar analysis for the sharp Tb3+ emission reveals a decreased emission in the 1
:
1 and 1
:
10 cases with respect to that observed in the Zn(Tb)S nanoparticles, whereas in the 1
:
10−2–1
:
10−3 cases the Tb3+ emission gets enhanced. In the 1
:
10−1 case, any change in the Tb3+ emission compared to that observed in the Zn(Tb)S nanoparticles is not evident. Clearly, competitive factors play a role and these factors are discussed in the following text. The data presented in Fig. 7 as average and standard deviation include variation from the independent synthesis of the Zn(Tb)S nanoparticles and subsequent post-synthetic modification. For [Zn(Tb)S]
:
[Pb2+] = 1
:
10−4–1
:
10−5, the trend in Tb3+ emission did not result in a trend with quantitative agreement and hence these data are not included. In these two samples, unfortunately we could not generate reproducible data. The non-reproducibility of the Tb3+ emission quantum yield might be associated with the difficulty in controlling the subtle electronic interactions between Tb3+ and the small amount of post-synthetically added Pb2+ from the post-synthetic treatment with an aqueous dispersion of the Zn(Tb)S nanoparticles prepared independently.
The photoluminescence excitation spectra (Fig. 6) of the different studied nanoparticles monitoring the broad emission band centered at 400 nm, in the cases where emission is prominent, reveal a broad band centered around 280 nm, which has been assigned to the band gap transition of the Zn(Tb)S nanoparticles. Excitation spectra were also acquired, monitoring the Tb3+ emission at 545 nm. These spectra provide information about the electronic structures that are responsible for generating the Tb3+ emission. The relevant spectral profile for the Zn(Tb)S nanoparticles reveals a broad band centered around 280 nm and most remarkably this profile is devoid of significant contributions from direct 4f–4f sharp excitation bands, suggesting the operation of an optical antenna effect. Moreover, in the post-synthetically modified nanoparticles (wherever Tb3+ emission is evident), the corresponding spectral profile conserves the general feature of broadness, suggesting the operation of an optical antenna effect to sensitize the Tb3+ luminescence in the nanoparticles studied.
It has been argued that with the variation of reactant concentration from [Zn(Tb)S]
:
[Pb2+] = 1
:
10−5–1
:
10, it is possible to access scenarios that involve low to heavily co-doped nanoparticles without significant contributions from ternary mixtures. Given the formation of a ternary mixture, (i) distinct terbium sulfide and lead sulfide phases should have been observed in the HRTEM and SAED patterns and (ii) the photoluminescence excitation spectrum, upon monitoring the Tb3+ emission at 545 nm, would have more contribution from the direct sharp intra-configurational 4f–4f bands due to the contribution from more surface related terbium atoms in the nanoparticles. As none of these effects have been clearly observed we exclude the possibility of formation of a ternary mixture at least in the relative reactant concentrations studied and emphasise the importance of the formation of co-doped nanoparticles.
The trend in the photoluminescence spectra combined with the elemental composition as determined from the EDS has been rationalized by the following processes.
:
Pb2+ and Tb3+
:
Pb2+ pairs. For the nanoparticles with higher [Zn(Tb)S]
:
[Pb2+], the characteristic broad ZnS based nanoparticles and sharp Tb3+ emission were both found to be present, suggesting that a lower relative [Pb2+] with [Zn(Tb)S]
:
[Pb2+] = 1
:
10−5 is unable to alter the composition of the Zn(Tb)S nanoparticles to a significant extent. With this reactant ratio being 1
:
10−4, the broad emission decreases by ∼30% in intensity, compared to that observed in the Zn(Tb)S nanoparticles. With a gradual increase in the relative amount of Pb2+, the broad emission characteristic of the ZnS based nanoparticles centered around 400 nm disappears significantly at around a nominal [Zn(Tb)S]
:
[Pb2+] = 1
:
10−3–1
:
10−1 and eventually with further increase in [Pb2+] to around a nominal [Zn(Tb)S]
:
[Pb2+] = 1
:
1 the characteristic sharp Tb3+ emission bands almost disappear, as evident from Fig. 6 and 7. The Tb3+ emission disappears completely with a nominal [Zn(Tb)S]
:
[Pb2+] = 1
:
10. It is remarkable to note that both the ZnS nanoparticle centered broad emission around 400 nm and the characteristic sharp Tb3+ emission bands at 490, 545, 585 and 620 nm were found to be absent in the emission spectrum in cases with a nominal [Zn(Tb)S]
:
[Pb2+] = 1
:
10. This suggests that the post-synthetic modification of the Zn(Tb)S nanoparticles with Pb2+ results in a complete displacement of the Zn2+ and Tb3+ from the nanoparticles, albeit with a greater ease for the Zn2+
:
Pb2+ pair compared to the Tb3+
:
Pb2+ pair. These findings are qualitatively consistent with the EDS measurements (vide supra). To summarize, the post-synthetic treatment of the Zn(Tb)S nanoparticles with Pb2+ having a nominal [Zn(Tb)S]
:
[Pb2+] = 1
:
10 or even 1
:
1 results in a complete or near complete (see Table S1†) displacement of Zn2+ and Tb3+, with the formation of PbS nanoparticles (vide supra).In short, the emission spectra with gradually increasing concentrations of Pb2+ allow identification of a trend that gauges the cation exchange reaction in the Zn(Tb)S nanoparticles. The potential candidates for the exchange pairs in the system investigated are Zn2+
:
Pb2+ and Tb3+
:
Pb2+, respectively. The observations presented provide a foundation for photoluminescence based detection of Pb2+ through monitoring the characteristic emission signatures related to ZnS and Tb3+ in the post-synthetically modified Zn(Tb)S nanoparticles. Moreover, the results obtained in the present work indicate that it is possible to access PbS, Pb(Tb)S, and Zn(Tb)(Pb)S through post-synthetic modification of Zn(Tb)S nanoparticles via the addition of Pb2+ solutions of various concentrations. This enables the tracking of photoluminescence characteristics from low to heavy co-doping and eventually the formation of a material of different chemical identity.
Another important avenue that is related to the cation exchange reaction in semiconductor nanoparticles is the reversibility of the reaction.4 In order to evaluate the possibility of such a reverse reaction, experiments have been undertaken in which the PbS nanoparticles, formed via the treatment of [Zn(Tb)S]
:
[Pb2+] = 1
:
1, were exposed to excess Zn2+ and Tb3+. Visually, the material changes color from brown to off-white suggesting a transformation in the composition of the material. Images of the materials along with the relevant photoluminescence excitation and emission spectra of initial Zn(Tb)S, PbS formed from the treatment of [Zn(Tb)S] : [Pb2+] = 1:1 (A), and (A) exposed to excess Zn2+ and Tb3+ precursors are shown in Fig. 8. The A/ZnPb sample clearly shows the broad blue and sharp emission of ZnS and Tb3+, respectively. This suggests that it is indeed possible to attain reversibility in the underlying cation exchange reaction. However, it is worth noting that the broad blue profile is red shifted in the reformed Zn(Tb)S nanoparticles, compared to that in the initial Zn(Tb)S nanoparticles. A difference in surface reconstruction might have a role in this spectral shift. Moreover, a comparison of the emission quantum yield in the initial and reformed Zn(Tb)S nanoparticles reveals a decrease of emission by 1.3 and 3.4 times for the ZnS and Tb3+ emission, respectively, upon the reverse cation exchange reaction.
To this end, it is worth including the aspects related to cation exchange in semiconductor nanoparticles involving Zn(Tb)S and Pb2+ as the reactant nanoparticles and post-synthetically added cation, respectively. Various previous studies revealed mechanistic insight about this fascinatingly fast reaction in semiconductor nanoparticles.2,4–7 Firstly, the exchange process does not affect the anionic network of the nanoparticles significantly, as is evident from the EDS data of the samples investigated. Secondly, as discussed above, based on the electron microscopy measurements we could not detect any faceted characteristics nor could we observe the partial exchange of cations. Thirdly, the efficiency of a cation exchange reaction is dependent on the solubility product constant of metal sulfides and the standard reduction potential of Mn+/M couples. A lower and higher value of these, respectively, would result in efficient cation exchange. Considering these physical parameters, it is justifiable to explain the cation exchange of component cations of Zn(Tb)S nanoparticles using either Pb2+, Hg2+ or Cd2+ separately (vide infra). Fourthly, the reversible nature of the exchange reaction could be rationalized using the hard soft acid base (HSAB) theory, especially from the hardness values of a given moiety. For example, the hardness values of Zn2+, Tb3+, Pb2+, C6H5OH and C6H5SH are 10.88, 14.35, 8.46, 4.8 and 4.6, respectively.33 In this tabulation, the values for C6H5OH and C6H5SH are included to closely mimic the value for 1-thioglycerol, the value of which was not accessible to us directly. Nonetheless, these values indicate that it would be possible to replace softer Pb2+ from PbS nanoparticles to reform Zn(Tb)S nanoparticles through reverse cation exchange.
:
[Pb2+] ≥ 1
:
1. However, even with [Zn(Tb)S]
:
[Pb2+] = 1
:
10−4, the broad emission of the ZnS nanoparticles has decreased intensity, compared to that observed in the Zn(Tb)S nanoparticles. Considering the presence of an appreciable amount of zinc and sulfur in these nanoparticles, the decrease of emission in these cases is not straightforward. It has been anticipated that the decreased blue emission in these cases is likely associated with the Pb2+ induced modifications of the surface properties of the nanoparticles or modulation of photoluminescence properties through the incorporation of Pb2+ in the interstitial sites of the Zn(Tb)S nanoparticles. The results presented here could not differentiate between these possibilities, as this requires detailed structural investigation and is beyond the scope of the current work.
:
[Pb2+] = 1
:
10−2–1
:
10−3. This observation is remarkable in light of a general research topic that aims to brighten the Ln3+ emission in a given system. Making a Ln3+ based luminophore bright enough to be practically useful is a challenging task due to the inefficient direct excitation (associated with the very low molar extinction co-efficient of Ln3+) and quenching of luminescence through environmental (ligand and/or solvent) factors.34,35 The current work does not identify the origin of the Tb3+ photoluminescence brightening at selected Pb2+ concentrations and this will be addressed in detail in future work. Possibilities might be associated with the structural modification of the nanoparticles at a particular [Pb2+], modulation of electronic factors, and tuning of surface properties, among others.In such a photophysical rationalization, it is important to identify the relative position of the Ln3+ ground and luminescent energy levels with respect to the valence and conduction bands of the host material. It has generally been observed that appreciable host sensitized Ln3+ emission could be realizable when the Ln3+ ground and luminescent energy levels are placed optimally above and below the valence and conduction bands of the host material. To construct such energy level schematics, we adopted the method proposed by Dorenbos and co-workers,38,39 in which the Ln3+ binding energy trend has been considered to be universal due to the core like features and the charge transfer energy between the anion valence band and Eu3+ ground state has been considered to be same as the energy difference between the valence band of the host material and the Eu2+ ground state. Moreover, by placing the Eu3+ ground state energy level at 5.7 eV lower than the Eu2+ ground state for lower band gap materials, like the materials investigated in the present work, and considering the universal relative binding energy trend of Ln3+, the entire relative energy level schematic can be constructed.
The relative energy level positions of the Tb3+ ground and luminescent energy levels with respect to the valence and conduction bands of the ZnS and PbS hosts are shown in Fig. 9. This schematic clearly identifies that while both the hosts are efficient in hole trapping at the Tb3+ ground energy level, the autoionization is expected to be very efficient in PbS and the same would be negligible in ZnS. Thus for sensitization of Tb3+ emission, ZnS would act as better host material, compared to that which could be realized from PbS based materials.
:
[Mn+] maintained at a 1
:
1 and 1
:
10−2 ratio. The choice of these concentration ratios was based on the corresponding Pb2+ case, with the exchange of both Zn2+ and Tb3+, and a representative case where Tb3+ emission enhancement was observed, respectively.
The trends in the broad and sharp emission of the ZnS nanoparticles and Tb3+, respectively, from these measurements with [Zn(Tb)S]
:
[Mn+] = 1
:
1 are summarized in Fig. 10, with the corresponding photoluminescence spectral profiles shown in Fig. S2–S4 (ESI†). For [Zn(Tb)S]
:
[Mn+] = 1
:
1, the data reveal a disappearance of both ZnS and Tb3+ emission characteristics in the Zn(Tb)S nanoparticles with post-synthetic modification of the nanoparticles using Hg2+. This observation is at least similar to the corresponding case with Pb2+ (vide supra). The extent of such a disappearance is less evident with the addition of Cd2+, showing a red shift in the emission spectral profile. This shift is most likely associated with the formation of a mixed phase in the nanoparticles, generating a contribution from lower band gap materials. Similar experiments with the addition of Ca2+, Mg2+, Na+ and K+ did not produce similar dramatic decreases in the luminescence of the Zn(Tb)S nanoparticles. In these cases, a marginal to significantly distinct decrease in the broad emission of the ZnS nanoparticles is noticeable with a consistent blue shift in the broad blue spectral band, which has been attributed to the subtle changes in the structure of the nanoparticles. These observations collectively indicate that it is indeed possible to detect heavy metals (Pb2+, Hg2+, and Cd2+) selectively using the post-synthetic modification of Zn(Tb)S nanoparticles. The nanoparticles where the metal ion is Ca2+, Mg2+, Na+ and K+ cause a change in the intensity of the sharp Tb3+ emission, compared to that observed in the Zn(Tb)S nanoparticles. An emission enhancement of Tb3+ in cases of post-synthetic modification with either Mg2+ or Na+ is noticeable, where an increase of emission by 1.1 and 1.3 times has been observed, respectively.
On the other hand, [Zn(Tb)S]
:
[Mn+] = 1
:
10−2 reveals a specific nature that is associated with Pb2+ among the cations investigated. These results are summarized in Fig. 11 and the corresponding spectra are shown in Fig. S5–S7 (ESI†). The reason behind this sort of specificity, while being unknown at this juncture, could be associated with the similar ionic radii of Tb3+ and Pb2+, being 118 and 119 pm, respectively. This reasoning awaits further detailed study and will be addressed independently. Moreover, for the cases with Ca2+, Mg2+, Na+ and K+, the broad ZnS emission decreases significantly with a blue shift in the blue emission band, suggesting that even a small amount of post-synthetically added cations tune the photophysical properties associated with the surface related emission in the Zn(Tb)S nanoparticles significantly. The emission enhancement in the cases with post-synthetic addition of either Mg2+ or Na+ is, however, not apparent.
To summarize, it is evident that control of the broad and sharp emission of ZnS and Tb3+, respectively, in the post-synthetically modified Zn(Tb)S nanoparticles is possible through varying the relative concentrations of reactants, with a dependence on the identity of the post-synthetically added cation. A comparative summary of the emission trend for the nanoparticles investigated in this work is provided in Table 1, clearly indicating that it is indeed possible to obtain a wide range of emission properties through simple chemical treatment of semiconductor nanoparticles under ambient conditions.
| System | [Zn(Tb)S] : [Mn+] |
[Zn(Tb)S/Mn+]Broad ZnS nanoparticles emission/[Zn(Tb)S]Broad ZnS nanoparticles emission | [Zn(Tb)S/Mn+]Sharp Tb3+ emission/[Zn(Tb)S]Sharp Tb3+ emission |
|---|---|---|---|
| Zn(Tb)S/Pb | 1 : 1–1 : 10 |
Diminishes | Diminishes |
1 : 10−1 |
Diminishes | Similar | |
1 : 10−2–1 : 10−3 |
Decreases significantly | Increases by 3–4 times | |
1 : 10−4–1 : 10−5 |
Decreases marginally to nearly similar | Did not produce data with quantitative agreement | |
| Zn(Tb)S/Hg | 1 : 1 |
Diminishes | Diminishes |
1 : 10−2 |
Diminishes | Diminishes | |
| Zn(Tb)S/Cd | 1 : 1 |
Decreases significantly with red shifted emission | Decreases significantly |
1 : 10−2 |
Decreases significantly with red shifted emission | Decreases significantly | |
| Zn(Tb)S/Ca | 1 : 1 |
Decreases with blue shifted emission | Decreases by 0.8 times |
1 : 10−2 |
Decreases with blue shifted emission | Decreases by 0.5 times | |
| Zn(Tb)S/Mg | 1 : 1 |
Decreases with blue shifted emission | Increases by 1.1 times |
1 : 10−2 |
Decreases with blue shifted emission | Decreases by 0.7 times | |
| Zn(Tb)S/Na | 1 : 1 |
Decreases marginally with blue shifted emission | Increases by 1.3 times |
1 : 10−2 |
Decreases with blue shifted emission | Decreases by 0.9 times | |
| Zn(Tb)S/K | 1 : 1 |
Decreases with blue shifted emission | Similar |
1 : 10−2 |
Decreases with blue shifted emission | Decreases by 0.3 times |
Overall, it has been argued that varying the ratio of Zn(Tb)S nanoparticles and Pb2+ in a range of six orders allows access to scenarios ranging from low to heavy doping levels and ultimately the synthesis of a material of a different chemical identity. Moreover, the enhancement of Tb3+ emission has been found to be Pb2+ specific in the range [Zn(Tb)S]
:
[Mn+] = 1
:
10−2–1
:
10−3; this led us to envisage the possibility that there exist subtle structural variations that correlate with the similar ionic radii of Tb3+ and Pb2+. With an equimolar or higher ratio for the concentration of the Zn(Tb)S nanoparticles and Pb2+, cation exchange plays a dominant role. This necessarily leads to the (i) decrease in the amount of Tb3+ due to the exchange of cations and (ii) lesser sensitization ability of PbS to generate the Tb3+ emission; both supporting a decrease of Tb3+ emission. It is important to note that realization of appreciable Tb3+ emission requires host sensitization due to its very low molar extinction co-efficient and the efficient environment induced quenching of Tb3+ luminescence.34,35 While these aspects satisfactorily identify the reason for Tb3+ emission decrease in the domain of cation exchange, the specific reason for Tb3+ emission enhancement at particular relative concentrations of Pb2+ is still not clearly identified. To this end, we wish to undertake a detailed time-resolved photoluminescence investigation of both the broad ZnS and sharp Tb3+ emissions, respectively, as a function of Pb2+ concentration to reveal the nature of the radiative and non-radiative rates in these systems. We, however, believe that such a study is beyond the scope of the current work, which mainly attempts to explore how the photophysical properties of the Zn(Tb)S nanoparticles change as a function of post-synthetically added Pb2+ and in cases with selected concentrations of other cations.
The use of cation exchange reactions to develop sensors for heavy metal ions and lead in particular has been attempted by few research groups.25,26 For example, Brock and co-workers developed a Pb2+ and Hg2+ sensor that is based on a cation exchange reaction from zinc sulfide nanoparticles and they quantified the process using inductively coupled plasma mass spectroscopy (ICP-MS).25 Chattopadhyay and co-workers demonstrated cation exchange reactions of Hg2+, Ag+ and Pb2+ from chitosan stabilized ZnS quantum dots towards the development of sensors of these cations and estimated a detection limit for Hg2+ that is in the range of ppm.26 Based on the demanding experimental procedure for ICP based measurements and the relatively easier realization of photoluminescence experiments with high sensitivity from the perspective of both instrumentation and feasibility of performing measurements in vivo, our aim was to develop a photoluminescence based sensor for biologically hazardous metal ions through the post-synthetic modification of inorganic nanoparticles. This approach collectively offers easy realization of both the chemical reaction and the measurement. Moreover, while most of the previous studies carried out the exchange reaction using undoped nanoparticles, we have attempted to perform such a reaction in the presence of two cations. The terbium cation incorporated zinc sulfide [Zn(Tb)S] nanoparticles were considered for this purpose, with the nanoparticles being treated with an appropriate metal nitrate salt post-synthetically. The strategy of performing the exchange reaction in the presence of two cations of diverse chemical nature provides a route to use the robustness of the cation exchange reaction in semiconductor nanoparticles. Additionally, the involvement of lanthanide cations (terbium in the present study) offers the possibility of time-gated measurements, a feature related to the longer (microseconds to milliseconds) photoluminescence lifetime of these cations. Moreover, in a given scenario with the occurrence of simultaneous cation exchange reactions, the experimental outcome also cross verifies the detection results.
The trend in the relative emission of the broad ZnS and sharp Tb3+ in the post-synthetically modified Zn(Tb)S nanoparticles as a function of [Pb2+] is shown in Fig. 12. The results presented indicate that based on a decrease of the broad emission of ZnS, it is possible to detect Pb2+ through monitoring the photoluminescence properties related to ZnS in the Zn(Tb)S nanoparticles, with a minimum concentration ratio of [Zn(Tb)S]
:
[Pb2+] = 1
:
10−4. Moreover, the feature of a Pb2+ induced increase in the Tb3+ emission could also be utilized to detect Pb2+ with a minimum concentration ratio of [Zn(Tb)S]
:
[Pb2+] = 1
:
10−3. A [Zn(Tb)S] of 0.3 mM was used in the present work for the electronic spectroscopy experiments. Correspondingly, the Tb3+ concentration was around 30 μM, considering the dopant ratio during the synthesis of the Zn(Tb)S nanoparticles and assuming complete incorporation of the dopants during the synthesis of the nanoparticles. Additionally, we note that a nanoparticle concentration in the order of tens of millimolar was required for the purification of the post-synthetically modified nanoparticles. Based on this, a Pb2+ detection capability of ∼0.2 ppm was estimated using the broad ZnS and sharp Tb3+ related emission characteristics separately in the post-synthetically modified Zn(Tb)S nanoparticles.
Moreover, the data in Fig. 12 clearly indicate a deviation from linear behavior. It is important to note that the nanoparticles in the present work have been modified using Pb2+ concentrations that vary by 106 in the order of magnitude and the discussion above discusses the different physical processes associated with the different concentration regimes. For example, for the broad ZnS emission, [Zn(Tb)S]
:
[Pb2+] < 1
:
1 will have a contribution from the structural modification of the nanoparticles, in the same way >1
:
1 measures cation exchange. For the sharp Tb3+ emission, [Zn(Tb)S]
:
[Pb2+] = 1
:
10−2–1
:
10−3 and >1
:
1 enable monitoring of the Tb3+ emission enhancement and cation exchange, respectively. Accordingly, it is anticipated that a deviation from linearity is not surprising.
At this juncture we note that while the use of Zn(Tb)S nanoparticles for the detection of Pb2+ in aqueous dispersions is not applicable to access the regulatory amount of <15 ppb set by the US Environmental Protection Authority (EPA),40 they would only be used for heavily contaminated samples. This difficulty is associated with the relatively low molar extinction co-efficient of the ZnS nanoparticles, being in the range of 103 M−1 cm−1. Nonetheless, the results presented in this work clearly show the vastness of the photoluminescence properties that evolve as a function of reactant concentration and direct the use of these properties for similar metal ion detection using other semiconductor nanoparticles with higher molar extinction co-efficients. However, an associated challenge remains in choosing a suitable host (semiconductor nanoparticles)–guest (Ln3+) combination,36 with appreciable host sensitized Ln3+ emission. Optimizing such a nanoparticle system for use in detecting even lower levels of Pb2+ is currently underway in our laboratory.
:
[Pb2+] ≥ 1
:
1 displacing both Zn2+ and Tb3+ from the Zn(Tb)S nanoparticles. The disappearance and emission enhancement of the broad ZnS related and sharp Tb3+ emission characteristics, respectively, provide an opportunity to detect Pb2+ with at least [Zn(Tb)S]
:
[Pb2+] = 1
:
10−4 and 1
:
10−3, respectively. In all the cases with Tb3+ emission evident, the nanoparticles were acting as an optical antenna to sensitize the Tb3+ emission. Performing similar experiments with other cations indicates the importance of the identity of the post-synthetically added cation and enables the detection of Hg2+ that is comparable to or better than that of Pb2+, with lesser detection efficiency for Cd2+. The corresponding cases with Ca2+, Mg2+, Na+, and K+ did not produce a similar decrease in the Zn(Tb)S nanoparticles emission characteristics, suggesting using the cation exchange strategy to sense heavy metals in general. However, the post-synthetically added Pb2+ induced Tb3+ emission enhancement has been found to be specific in nature, at least among the cations investigated. However, cations like Mg2+ and Na+ when post-synthetically added have been found to enhance the Tb3+ emission in the Zn(Tb)S nanoparticles. This feature is attractive to a general research area that is associated with increasing lanthanide cation emission, a challenging task related to the extremely low molar extinction co-efficients of these cations. From the acquired spectra, the detection capability for Pb2+ has been estimated as ∼0.2 ppm using either the broad or sharp emission of ZnS and Tb3+, respectively, in the post-synthetically modified Zn(Tb)S nanoparticles. The associated physical processes are guided by the structural modifications and Tb3+ emission enhancement in the Zn(Tb)S nanoparticles, respectively. Finally, the use of trivalent lanthanide cations (Tb3+ in the present work) ensures the accessibility of time-gated measurements that are associated with longer (microseconds to milliseconds) luminescence lifetimes, further increasing the detection sensitivity using the lanthanide luminescence. Collectively, the data obtained in the present work provide a foundation to use the emission characteristics of post-synthetically modified semiconductor nanoparticles to detect heavy metal cations in general and lead in particular in aqueous dispersions using the wide range of photoluminescence characteristics accessible through varying the relative concentrations of the reactants and the identity of the post-synthetically added cation.
Footnote |
| † Electronic supplementary information (ESI) available: Representative EDS, elemental composition, and photoluminescence spectra of the nanoparticles are presented. See DOI: 10.1039/c8ra02403k |