Open Access Article
This Open Access Article is licensed under a
Creative Commons Attribution 3.0 Unported Licence

One-pot synthesis of ultrafine amphiphilic Janus gold nanoparticles by toluene/water emulsion reaction

Kun Luo*a, Chengliang Hua, Yujia Luob, Degui Lia, Yongdong Xianga, Yuanying Mua, Haiming Wanga and Zhihong Luoa
aCollege of Materials Science and Engineering, Guilin University of Technology, 12 Jiangan Road, Guilin 541004, P. R. China. E-mail: luokun@glut.edu.cn
bThe First Hospital of China Medical University, 155 Nanjing Street, Heping District, Shenyang 10122, P. R. China

Received 17th September 2017 , Accepted 31st October 2017

First published on 6th November 2017


Abstract

Ultrafine amphiphilic Janus gold nanoparticles (Au NPs, d ≈ 2.1 nm) were synthesized in batch by the emulsion reaction between chlorotriphenylphosphine gold(I) in toluene and tetrakis(hydroxymethyl)phosphonium chloride in alkaline solution, followed with phase inversion by adding excess toluene, resulting in a yielding rate of up to 93.3%. FT-IR, Raman, TG and XPS analyses indicate that the emulsion reaction product is composed of Au NPs protected by triphenylphosphine, tris(hydroxymethyl)phosphine and their oxides. A NOESY experiment indicates that these ligands are separated into hydrophilic and lipophilic compartments on the individual Au NPs. The Janus wettability of the thin films by the static toluene/water interfacial reaction and Langmuir re-assembly of the as-dispersed emulsion reaction product suggests that spontaneous phase separation of capping ligands occurs with the formation of the Au NPs at the toluene/water interface, which can be maintained even in the colloidal state. The scalable one-pot synthesis of the amphiphilic Janus Au NPs allows further functionalization for the diagnosis and therapy of cancers and biphasic catalysis at low cost.


1. Introduction

Gold nanoparticles (Au NPs) have been recognized as attractive candidates for the diagnosis and therapy of disease.1–4 The absorbance and fluorescence can be tuned to the near-infrared region by altering the size and morphology of Au NPs, where body tissues absorb weakly and hence allow some optical applications in vivo, including optical imaging5 and photothermal6 or radio therapy.7 The high atomic index and electron density of Au NPs are also beneficial for the efficient absorption of X-ray radiation, which lead to a better contrast for CT and MRI than the conventional iodine-based agents.5,8 Moreover, the excellent biocompatibility, chemical stability and low toxicity allow Au NPs to serve as prospective targeting delivery agents into tumour cells by the effect of permeability and retention (EPR),9 where drug molecules can be released by external stimuli (such as pH,10,11 temperature,12 light13 or competitive molecules). In this aspect, drug molecules are either covalently conjugated onto Au NPs,14–16 or encapsulated in Au-NP-stabilized Pickering emulsions.17,18 In the latter case, ultrafine Au NPs are used to build up nanoscale micellar vehicles, which can provide with large loading capacity and multiple drug cargos into tumour cells. For example, nanomicelles encapsulated (in size from 22 nm to 48 nm) by amphiphilic Au NPs with polycaprolactone and methoxypoly(ethylene glycol) were reported to carry a model drug, 5-fluorouracil, where the drug release could last for more than 4 days.17,19

However, homogeneous nanoparticles (d < 10 nm) normally suffer from unstable adsorption at oil/water interfaces, which rely heavily on contact angles: at ca. 0° (or 180°), the desorption energy of NPs at the interface is only 1/3000 of the one at 90°, in which case the interfacial adsorption can hardly stand thermal fluctuations.20 Research has shown that amphiphilic Janus NPs exhibit ca. 3-fold desorption energy of the homogeneous counterparts at immiscible liquid/liquid interfaces,21 which can stay at the interfaces even at a contact angle of 0° (or 180°). Efforts have been paid on the interface engineering of homogeneous NPs. To avoid the possible overturn during surface modification, Pradhan et al.22,23 assembled the hexanethiolate-protected Au NPs (d ≈ 2 nm) into a Langmuir film, which was then immersed in the 2-(2-mercapto ethoxy)ethanol solution, resulted in amphiphilic Janus Au NPs after ligand exchange in part. Xu et al. simplified the operation,24 where the precursor octanethiolate-protected Au NPs (d ≈ 5 nm) were compressed to form a Langmuir film, but the ligand exchange was triggered by the injection of 3-mercaptopropane-1,2-diol into the water underneath without removal of the film.

Andala et al.25 reported that the immiscible liquid/liquid interface facilitates the spontaneous phase separation between hydrophilic and hydrophobic ligands, where the ligand substitution of dodecylamine on the precursor Au NPs (d ≈ 9.2 nm) by mercaptoundecanoic acid and dodecanethiol at the toluene/water interface directly led to the formation of amphiphilic Janus Au NPs, no matter the thiol ligands were introduced simultaneously or one-by-one into the system, since the adsorption of amphiphilic particles localized at the interface is thermodynamically more favorable than those with mixed ligands. Inspired by the approach, a series of phosphine-modified amphiphilic Janus Au NPs ranging from 2 nm to 18 nm were synthesized by ligand exchange at toluene/water interface in our previous work.26 Moreover, Kim et al. recently demonstrated that the spontaneous phase separation was also possible to occur in a single solvent,27 where Janus Au NPs (d ≈ 2 nm) were successfully synthesized in toluene, based on the balance between the enthalpy of phase separation and conformational entropy between the two ligands of hexadecane-1-thiol and 1,1′,4′,1′′-terphenyl-4-thiol. In this study, spontaneous phase separation of capping ligands was also noticed to occur on the Au NPs of the interfacial reaction product between chloro(triphenyl)phosphine gold (Au(PPh3)Cl) in toluene and tetrakis(hydroxymethyl)-phosphonium chloride (THPC) in alkaline solution, and the large toluene/water emulsion interface was used to synthesize ultrafine amphiphilic Janus Au NPs in batch, followed with phase inversion by adding excess toluene, leading to the batch production with a yielding rate of up to 93.3% at low cost. In addition, the Janus Au NPs are stable in colloidal state, and allow further functionalization for the possible applications on targeting drug delivery, tumor imaging and biphasic catalysis.

2. Experimental

2.1 Materials and chemicals

Gold wire (99.99%, d = 0.5 mm), triphenylphosphine (PPh3, CP) and toluene (99.5%, AR) were from Sinopharm Chemical Reagent Co. Ltd., China. Acetonitrile (CH3CN, 99.5%, AR), ether (99.8%, AR), dichloromethane (CH2Cl2, 99.5%, AR), acetone (99.5%, AR), pentane (99%, AR), dimethyl formamide (DMF, 99.5%, AR), hydrochloric acid (HCl, 36–38%, AR) and sodium hydroxide (NaOH, 96%, AR) were purchased from Shantou Xilong Chemicals Co. Ltd., China. Tetrakis(hydroxymethyl)phosphonium chloride (THPC, CP, 80%) was from Tokyo Chemical Industry Co. Ltd., Japan. Deionized water (18.2 MΩ cm) was employed to prepare the aqueous solutions in the experiments.

Chloro(triphenyl)phosphine gold (Au(PPh3)Cl) was synthesized electrochemically following a method described by Huang et al.28 Typically, 0.95 mL of HCl was added dropwise into 15 mL CH3CN in a vial, followed with the dissolution of 0.092 g PPh3. Au wire and platinum plate served as the anode and cathode, respectively. White deposit was produced on the bottom when a voltage of 2.0 V was applied for 6 h, which was filtered and rinsed with ether till it appeared pure white. After drying at 60 °C, the white powders were dissolved again in 1.5 mL of CH2Cl2, and re-crystallization was carried out at −10 °C as 10 mL of pentane was added. The crystals were again rinsed with pentane and dried at 60 °C, leading to the Au(PPh3)Cl powders.

2.2 Synthesis of amphiphilic Janus Au NPs

50 mL of 1.5 mM Au(PPh3)Cl toluene solution and 80 mL of 31.25 mM NaOH solution were mixed with an emulsifying mixer in an Erlenmeyer flask at a rate of 4000 rpm, followed with the dropwise injection of 1.65 mL of 50 mM THPC solution to trigger the toluene-in-water emulsion reaction. After 3 h of reaction, additional 50 mL of toluene was injected into the flask with stirring for phase inversion, and the water-in-toluene emulsion reaction was fulfilled after another 2 h. Then, the emulsion mixture was removed in a separatory funnel and kept still overnight, where the product at the toluene/water interface was collected, and then rinsed by centrifuging with acetone and deionized water for three times, respectively, resulting in yellowish powders after freeze drying. Colloids of the Au NPs in the emulsion reaction product were prepared by ultrasonic dispersion in DMF, which were available for further characterizations.

2.3 Analysis of Au(PPh3)Cl concentration in toluene

The reduction rate from Au(PPh3)Cl to amphiphilic Janus Au NPs in the emulsion reaction was calculated by the following equation:
 
image file: c7ra10323a-t1.tif(1)
where Ci and Cf are the initial and final concentrations of Au(PPh3)Cl in toluene in the emulsion reaction. In the measurement, 5 mL of the sample toluene solution was injected in a silica beaker (150 mL), which was dried on an electric hot plate to remove the toluene slowly. Then, the evaporated residual was heated at 200 °C for 0.5 h and calcined at 800 °C for 20 min. The obtained yellowish residual was removed into the silica beaker, 0.1 mL of 10% KCl solution and 10 mL of aqua regia were added in sequence to re-dissolve the residual, which was dried on the electric hot plate. The final residual was dissolved again with 10 mL aqua regia, which was diluted with deionized water in a volumetric flask (100 mL), which was available for the gold content analysis. The Ci and Cf were determined by an atomic absorption spectrophotometer (AAS, TAS-986F, Beijing Puxi Universal Instruments Co, Ltd.).

2.4 Wetting property of the thin film assemblies of Au NPs

To investigate the phase separation of the phosphine ligands, the wetting property of the Au-NP thin film assemblies were examined. On the one hand, a thin film was prepared by the static toluene/water interfacial reaction according to our previous work,29 where 8 mL of 31.25 mM NaOH solution and 5 mL of 1.5 mM Au(PPh3)Cl toluene solution were added in turn into a vial, followed with the injection of 165 μL of 50 mM THPC solution to trigger the reaction. After 24 h of reaction, a yellowish thin film was formed at the toluene/water interface. On the other hand, 1.0 mg of the emulsion reaction product was dispersed in 10 mL DMF by ultrasonic stirring, led to a colloid containing 0.1 mg mL−1 Au NPs. 3 mL of the colloid were spread on the water surface in a Langmuir trough (JML04C1-P, length × width × height = 21 cm × 8 cm × 0.8 cm, Shanghai Zhongchen Digital Technology Co. Ltd.). Langmuir films were produced as the pressure of 10 mN m−1 was applied on the floating Au NPs.

The above thin film assemblies were collected by clean glass slides: the slide moving upstroke from the water lifted the film up, which flipped over and left the lipophilic side up; while the slide moved downstroke to press the film into the water, which also flipped over and let the hydrophilic side up. The collected films were rinsed with acetone and deionized water, respectively, and were available for contact angle measurement after drying in ambient temperature. The contact angles of water droplets on the two surfaces were measured by a contact angle analyzer (JWA-360A, Xiamen Congda Smart Technology Co. Ltd.).

2.5 Characterizations

The morphology of the emulsion reaction product was characterized by a transmittance electron microscope (TEM, JEM-2010 JEOL, operated at 200 kV) and a field emission scanning electron microscope (SEM, S-4800, Hitachi, operated at 15 kV). UV-vis spectrophotometer (TU1901, Beijing Puxi Universal Instruments Co, Ltd.) was used to differentiate the emulsion reaction product and the Au-NP DMF colloid by the position of maximum absorbance, with a clean glass slide and a cuvette with pure DMF as reference, respectively. A Fourier transmittance infrared spectroscope (Thermo Nexus 470 FT-IR), a confocal Raman microscope (DXR, Thermo Scientific, at 532 nm), a thermogravimetric analyzer (Q-500, Thermal Analysis Instruments) and an X-ray photoelectron spectroscope (XPS, AXIS ULTRA XPS, KRATOS) were employed to determine the capping ligands of the emulsion reaction product.

The nuclear Overhauser enhanced spectroscopy (NOESY) was also employed to investigate the phase separation of the ligands on the Au NPs in the emulsion reaction product. NOESY is accepted as a phase-sensitive two-dimensional NMR technique, which can differentiate the amphiphilic Janus NPs from the homogeneous counterparts by detecting the distance-dependent nuclear Overhauser effect between proton spins. In the experiment, 25 mg of the emulsion reaction product were dispersed in 0.6 mL CDCl3, whose 1H and NOESY spectra were collected by an AV-400 MHz NMR Instruments (Bruker, Karlsruhe, Germany).

3. Results and discussion

3.1 Morphology of the emulsion reaction product

In our previous work, the static interfacial reaction between the Au(PPh3)Cl in toluene and THPC in alkaline solution resulted in the formation of a thin film assembly of Au NPs at the interface, and the Au NPs were found to be modified with the cleavage products of the reactants, i.e. tris(hydroxymethyl)phosphine (THP), triphenylphosphine (PPh3) and their oxides as well as small amount of Au(PPh3)xCl (x = 1 or 2).29 In this work, the large interface area of toluene/water emulsion drops was used to prepare the Au NPs in batch, accompanied with the phase inversion from toluene-in-water to water-in-toluene emulsions by the addition of excess toluene, in order to make effective use of Au(PPh3)Cl. The analysis of atomic absorption spectroscopy shows that the initial and final concentrations of Au(PPh3)Cl in toluene were 1.5 mmol L−1 and 0.1 mmol L−1, respectively, i.e. 93.3% of Au(PPh3)Cl was reduced in the emulsion reaction.

Fig. 1a shows the morphological evolution of emulsion droplets during the reaction under optical microscope: at the first 10 min of emulsion reaction, the droplets appear pretty round, but at 60 min some of them present with “wrinkled” surfaces, indicative of the formation of Au-NP thin film assemblies at the emulsion interfaces, which encapsulate the droplets in the case that some of the inner liquid is gone under the strong stirring. The lost liquid may coalesce to form new toluene-in-water emulsion droplets by stirring, so more deformed micellar assemblies are observed at 3 h of reaction. After the addition of excess toluene, different sized droplets and thin film fragments are seen in the picture at 5 h of reaction, indicative of the breakage of the films covering the toluene-in-water emulsion droplets, as well as the formation and coalescence of the Au-NP films on the water-in-toluene emulsion droplets.


image file: c7ra10323a-f1.tif
Fig. 1 Characterizations of the emulsion reaction product: (a) morphological evolution of the emulsion drops with reaction time at 10 min, 60 min, 3 h and 5 h under optical microscope; (b) SEM micrograph of the product; (c) TEM (left), HRTEM (upper right) and SAED (lower right) images of the product, and the inset shows the size distribution of Au NPs; (d) UV-vis spectra of the emulsion reaction product (lower image) and the as-dispersed Au NPs (upper image).

Fig. 1b shows the SEM micrograph of the reaction product, which is composed of film fragments produced by the dynamic stirring and phase inversion. As the product is further enlarged in the TEM image (Fig. 1c), the film fragments are actually consisted of regularly self-assembled Au NPs in an average diameter of 2.1 ± 0.6 nm (N = 307, shown in the inset). The HRTEM and the select area electron diffraction (SAED) displayed in the upper and lower right of Fig. 1c demonstrate that the Au NPs are in form of nanocrystals.

Fig. 1d presents the UV-vis spectra of the emulsion reaction product and its dispersion in DMF, in which the ultrasonic dispersion in DMF manifests a strong resonance peak at 538 nm corresponding to the absorption of colloidal Au NPs. In comparison, the emulsion reaction product presents a wide band at ca. 580 nm, and the red shift of absorbance is associated with the dipolar–dipolar interaction between the Au NPs in the thin film assembly, in line with previous literature.29,30 It was also noticed that the dispersibility of the emulsion reaction product relied heavily on the property of organic solvents: the emulsion reaction product could be dispersed in chloroform, THF and DMF, but in acetone or ethanol no peak shift was examined (not shown).

3.2 Composition of the capping ligands

Fig. 2a is the FT-IR spectrum of the emulsion reaction product. The band at 3429 cm−1 can be assigned to the O–H stretch, and the absorbance at 1632 cm−1 corresponds to the stretching of benzene ring in aromatic compounds. The peak at 1373 cm−1 is probably originated from the deformation of P[double bond, length as m-dash]O stretch, and the bands at 1123 cm−1 and 1034 cm−1 are likely attributed to the P–Ar stretch and C–O stretch in primary aliphatic alcohols. The broad band at 568 cm−1 attributes to the in-plane and out-of-plane ring deformation of benzene derivatives. The Raman spectrum in Fig. 2b exhibits four major bands. The band at 2842 cm−1 represents the C–H antisymmetric and symmetric stretching of the –CH2– in aliphatic compounds, and the peak at 1590 cm−1 is attributed to the benzene ring stretch in aromatic compounds. The bands at 1367 cm−1 and 570 cm−1 are likely attributed to the P[double bond, length as m-dash]O stretch and P–C stretch, respectively. Hence, both the FT-IR and Raman analyses suggest the presence of the cleavage products on the as-synthesized Au NPs, i.e. tris(hydroxymethyl)phosphine (THP), triphenylphosphine (PPh3) and their oxides.
image file: c7ra10323a-f2.tif
Fig. 2 FT-IR (a) and Raman (b) analyses of the emulsion reaction product.

The XPS survey was also employed to investigate the emulsion reaction product. Fig. 3a shows the fitted peaks for the C1s signal at 284.8 eV, 285.5 eV and 286.6 eV, corresponding to the C–C of benzene ring, C–OH and C[double bond, length as m-dash]O bonds. For the resolved O1s signal, three fitted peaks are observed at 530.5 eV, 531.4 eV and 532.2 eV in Fig. 3b, assigned to the groups of P[double bond, length as m-dash]O, C–OH and C[double bond, length as m-dash]O. The fitting of the resolved P2p peak ends up with five peaks at 130.8 eV, 131.6 eV, 132.2 eV, 133.2 eV and 134.4 eV as displayed in Fig. 3c, corresponding to the composition of PPh3, THP, PPh3O, THPO and Au(PPh3)Cl, respectively. As for the Au4f signal, two major fitted peaks appear at 83.9 eV and 87.6 eV in Fig. 3d, which can be assigned to the Au4f7/2 and Au4f5/2 of metallic gold. A small peak at 85.0 eV attributed to Au4f7/2+ (<2.9 at%) is also present, indicative of the existence of Au(PPh3)xCl (x = 1 or 2), in agreement with the analysis of P2p. The possible ligand composition from XPS analysis is listed in Table 1, which demonstrates that the atomic ratio of the lipophilic molecules (PPh3 and PPh3O) to the hydrophilic ligands (THP and THPO) is at about 0.94.


image file: c7ra10323a-f3.tif
Fig. 3 XPS analysis of the emulsion reaction product: (a) fitting of C1s signal; (b) fitting of O1s signal; (c) fitting of P2p signal; (d) fitting of Au4f signal.
Table 1 XPS analysis of the emulsion reaction product
Elements B. E. (eV) FWHM (eV) Atomic percentage (%) Possible chemistry
C1s 284.8 1.19 84.09 C–C (benzene ring)
285.5 1.15 14.65 C–OH
286.6 0.89 1.26 –C[double bond, length as m-dash]O
O1s 530.5 1.38 21.88 O[double bond, length as m-dash]P–
531.4 1.18 63.60 C–OH
532.2 0.98 14.52 –C[double bond, length as m-dash]O
P2p 130.8 0.74 28.67 PPh3
131.6 0.5 14.03 THP
132.2 0.71 18.07 PPh3O
133.2 1.34 35.64 THPO
134.4 0.95 3.59 Au(PPh3)Cl
Au4f 83.9 1.02 53.03 Au4f7/20
85.0 0.98 2.87 Au4f7/2+
87.6 1.09 44.10 Au4f5/20


Fig. 4 displays the thermogravimetric analyses of the emulsion reaction product. There is no visible weight loss at the temperature lower than 100 °C, indicative of a dry and stable sample. A weight loss of 26% appears in the TG curve at the range from 100 °C to 200 °C, where the DTG curve shows three endothermic processes probably attributing the release of incorporated solvents (toluene) and excess ligand molecules (THP, THPO, PPh3 or PPh3O). 5.6% of the weight is lost in the range from 200 °C to 400 °C, corresponding to the thermal cleavage of THP and THPO to phosphates, and the 12.3% weight loss from 400 °C to 780 °C is likely assigned to the degradation of PPh3 and PPh3O. The atomic ratio of the lipophilic (PPh3 and PPh3O) to hydrophilic (THP and THPO) groups is estimated as ca. 1.1 from the pyrolytic data of thermal degradation. Both the XPS survey and TG analysis indicate that the hydrophilic and the similar amount of lipophilic ligands are present on the Au NP's surface in the emulsion reaction product.


image file: c7ra10323a-f4.tif
Fig. 4 Thermogravimetric (TG and DTG) analysis of the emulsion reaction product.

3.3 Distribution of the capping ligands

NOESY is a phase-sensitive two-dimensional NMR technique, and has been employed to differentiate Janus nanoparticles from the homogeneous counterparts by detecting the distance-dependent nuclear Overhauser effect between proton spins.22 As shown in Fig. 5, the 1H NMR spectrum of the emulsion reaction product dispersed in CDCl3 presents five peaks, where the peaks at 0.85 ppm and 1.27 ppm are likely attributed to the methylene and hydroxyl protons of THP and THPO or their derivatives, and the strong peak at 1.56 ppm is assigned to the proton in H2O. The peak at 7.26 ppm is corresponding to the solvent CDCl3, and the one at 7.52 ppm is assigned to the protons in PPh3 and/or PPh3O. The diagonal profile in the NOESY spectrum in Fig. 5 indicates the interchain interactions on the Au NPs, which are arisen from the adjacent protons of the hydrophilic molecules (square and triangle) and lipophilic molecules (circle). The absence of signals in the reverse diagonal suggests that the interactions between the protons of THP/THPO and the ones of PPh3/PPh3O can be ignored, demonstrating that the hydrophilic (THP/THPO) and the lipophilic (PPh3/PPh3O) ligands actually situate on two separate compartments of the Au NPs' surface.
image file: c7ra10323a-f5.tif
Fig. 5 1H NMR and NOESY analyses of the emulsion reaction product.

To further understand the phase separation on the Au NPs, the wetting properties on the two surfaces of Au-NP thin film assemblies were also tested, where two kinds of samples were used in the experiment: (1) thin films synthesized by the static toluene/water interfacial reaction with the same recipe as the emulsion reaction; (2) Langmuir re-assemblies of the as-dispersed emulsion reaction product. Fig. 6a shows the pressure-area isotherm for the formation of Langmuir re-assembly of the as-dispersed emulsion reaction product. As the colloidal Au NPs were compressed in the Langmuir trough, the re-assembly of the Au NPs was prompted on the water surface, during which the structure of the floating Au NPs varied from the gaseous (G) phase, transition (gas–liquid, L–G) state, liquid (L) phase to the solid phase (S, i.e. Langmuir film) as marked in the graph, as the pressure increased from 6.8 mN m−1 to 25.8 mN m−1. Hence, the Langmuir re-assembly for contact angle measurement was prepared at the pressure of 10 mN m−1. The inset of Fig. 6a shows the way of collecting samples by the upstroke or downstroke movement of glass slides, which was also applied for collecting the films by the toluene/water interfacial reaction. In the latter case, the film located at the toluene/water interface, and the collection had to pass through the upper toluene layer in the system.


image file: c7ra10323a-f6.tif
Fig. 6 Janus wettability of the Au-NP thin film assemblies: (a) Langmuir re-assembly and sample collection of the as-dispersed emulsion reaction product; (b) contact angles on the two surfaces of the thin film by toluene/water interfacial reaction and the Langmuir re-assembly of the as-dispersed emulsion reaction product.

Fig. 6b illustrates that the contact angles on the two surfaces of the film by the interfacial reaction are determined as 68.5° and 18.7°, and the ones for the Langmuir re-assembly are 61.5° and 20.5°, respectively. The Janus wettability on the two surfaces of the thin film by the toluene/water interfacial reaction suggests that spontaneous phase separation of capping ligands occurred with the formation of the Au NPs at the toluene/water interface, owing to the constraint of the immiscible liquid/liquid interface, the biphasic supply and different affinity of ligand molecules. The Langmuir re-assembly of the as-dispersed Au NPs also present different wettability on the two surfaces, indicating that the Au NPs of the emulsion reaction product are still Janus amphiphiles in the colloidal state, which allow further functionalization for the prospective applications on targeting drug delivery, tumor imaging and biphasic catalysis. The ultrafine amphiphilic Janus Au NPs can be safely stored at ambient temperature, and the one-pot synthesis allows scalable production of amphiphilic Janus Au NPs at low cost.

4. Conclusion

Ultrafine amphiphilic Janus Au NPs were synthesized in batch by the emulsion reaction between Au(PPh3)Cl in toluene and THPC in alkaline solution, followed with phase inversion to make effective use of Au(PPh3)Cl, led to a facile and scalable approach at a yielding rate of up to 93.3%. TEM and UV-vis analyses indicate that the product are composed of Au nanocrystals with average diameter of 2.1 nm, and can be dispersed in organic solvents like DMF, THF and chloroform. FT-IR, Raman, XPS and TG analyses demonstrate that the Au NPs in the product are protected with lipophilic ligands (PPh3 and PPh3O) and the similar amount of hydrophilic molecules (THP and THPO). The NOESY experiment further demonstrate that the capping ligands of the individual Au NPs in the product are separated into the hydrophilic and lipophilic compartments, and the surface chemistry keeps stable for the as-dispersed Au NPs in DMF. The facile batch production of the amphiphilic Janus Au NPs allows prospective applications on targeting drug delivery, tumor imaging and biphasic catalysis at low cost. More efforts are under way on encapsulating anticancer drugs and tailoring the morphology of the Au-NP microcapsules.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

We grateful acknowledge the support from the National Natural Science Foundation of China (No. 21163004), Guangxi Natural Science Foundation (No. 2016GXNSFAA380107 and 2013 GXNSFAA019029), and the funding from the Collaborative Center for Exploration of Hidden Nonferrous Metal Deposits and Development of New Materials in Guangxi, and Guangxi Key Laboratory of Universities for Clean Metallurgy and Comprehensive Utilization of Nonferrous Metal Resources.

References

  1. G. De Crozals, R. Bonnet, C. Farre and C. Chaix, Nano Today, 2016, 11, 435–463 CrossRef CAS .
  2. K. M. Harkness, B. N. Turner, A. C. Agrawal, Y. Zhang, J. A. McLean and D. E. Cliffel, Nanoscale, 2012, 4, 3843–3851 RSC .
  3. I. Brigger, C. Dubernet and P. Couvreur, Adv. Drug Delivery Rev., 2002, 54, 631–651 CrossRef CAS PubMed .
  4. M. Srinivasan, M. Rajabi and S. A. Mousa, Nanomaterials, 2015, 5, 1690–1703 CrossRef CAS PubMed .
  5. T. Dreifuss, O. Betzer, M. Shilo, A. Popovtzer, M. Motiei and R. Popovtzer, Nanoscale, 2015, 7, 15175–15184 RSC .
  6. P. P. Yang, Y. G. Zhai, G. B. Qi, Y. X. Lin, Q. Luo, Y. Yang, A. P. Xu, C. Yang, Y. S. Li, L. Wang and H. Wang, Small, 2016, 12, 5423–5430 CrossRef CAS PubMed .
  7. L. Mocan, C. Matea, F. A. Tabaran, O. Mosteanu, T. Pop, T. Mocan and C. Iancu, Int. J. Nanomed., 2015, 10, 5435–5445 CAS .
  8. A. J. Mieszawska, W. J. Mulder, Z. A. Fayad and D. P. Cormode, Mol. Pharmaceutics, 2013, 10, 831–847 CrossRef CAS PubMed .
  9. M. X. Yu and J. Zheng, ACS Nano, 2015, 9, 6655–6674 CrossRef CAS PubMed .
  10. H. Cao, Y. Yang, X. Chen and Z. Shao, Nanoscale, 2016, 8, 6754–6760 RSC .
  11. N. Amreddy, R. Muralidharan, A. Babu, M. Mehta, E. V. Johnson, Y. D. Zhao, A. Munshi and R. Ramesh, Int. J. Nanomed., 2015, 10, 6773–6788 CAS .
  12. X. Niu, F. Ran, L. Chen, G. J.-E. Lu, P. Hu, C. P. Deming, Y. Peng, M. D. Rojas-Andrade and S. Chen, Langmuir, 2016, 32, 4297–4304 CrossRef CAS PubMed .
  13. A. G. Skirtach, A. Munoz Javier, O. Kreft, K. Kohler, A. Piera Alberola, H. Mohwald, W. J. Parak and G. B. Sukhorukov, Angew. Chem., Int. Ed. Engl., 2006, 45, 4612–4617 CrossRef CAS PubMed .
  14. S. Rana, A. Bajaj, R. Mout and V. M. Rotello, Adv. Drug Delivery Rev., 2012, 64, 200–216 CrossRef CAS PubMed .
  15. W. P. Savarimuthu, P. Gananathan, A. P. Rao, E. Manickam and G. Singaravelu, J. Nanosci. Nanotechnol., 2015, 15, 5577–5584 CrossRef CAS PubMed .
  16. M. Raoof, S. J. Corr, W. D. Kaluarachchi, K. L. Massey, K. Briggs, C. H. Zhu, M. A. Cheney, L. J. Wilson and S. A. Curley, Nanotechnology, Biology and Medicine, 2012, 8, 1096–1105 CrossRef CAS PubMed .
  17. S. Aryal, S. Pilla and S. Gong, J. Nanosci. Nanotechnol., 2009, 9, 5701–5708 CrossRef CAS PubMed .
  18. Y. Liu, J. J. Yin and Z. H. Nie, Nano Res., 2014, 7, 1719–1730 CrossRef CAS .
  19. H. Mitomo, K. Niikura and K. Ijiro, Kobunshi Ronbunshu, 2016, 73, 147–156 CrossRef CAS .
  20. A. Boker, J. He, T. Emrick and T. P. Russell, Soft Matter, 2007, 3, 1231–1248 RSC .
  21. B. P. Binks and P. D. I. Fletcher, Langmuir, 2001, 17, 4708–4710 CrossRef CAS .
  22. S. Pradhan, L. Brown, J. Konopelski and S. Chen, J. Nanopart. Res., 2009, 11, 1895–1903 CrossRef CAS .
  23. S. Pradhan, L. Xu and S. Chen, Adv. Funct. Mater., 2007, 17, 2385–2392 CrossRef CAS .
  24. Q. A. Xu, X. W. Kang, R. A. Bogomolni and S. W. Chen, Langmuir, 2010, 26, 14923–14928 CrossRef CAS PubMed .
  25. D. M. Andala, S. H. R. Shin, H. Y. Lee and K. J. M. Bishop, ACS Nano, 2012, 6, 1044–1050 CrossRef CAS PubMed .
  26. K. Luo, Y. Xiang, H. Wang, L. Xiang and Z. Luo, J. Mater. Sci. Technol., 2016, 32, 733–737 Search PubMed .
  27. S. Kim, T.-H. Kim, J. Huh, J. Bang and S.-H. Choi, ACS Macro Lett., 2015, 4, 417–421 CrossRef CAS .
  28. T. Huang, K. Luo, H. Huang, X. Li and Q. Zeng, Precious Met., 2012, 33, 14–17 CAS  , (in Chinese).
  29. K. Luo, S. L. Schroeder and R. A. Dryfe, Chem. Mater., 2009, 21, 4172–4183 CrossRef CAS .
  30. C. N. R. Rao, G. U. Kulkarni, P. J. Thomas, V. V. Agrawal and P. Saravanan, J. Phys. Chem. B, 2003, 107, 7391–7395 CrossRef CAS .

This journal is © The Royal Society of Chemistry 2017