Open Access Article
This Open Access Article is licensed under a
Creative Commons Attribution 3.0 Unported Licence

Electromagnetic and wave absorbing properties of Fe-doped polymer-derived SiCN ceramics

Youzhi Wangab, Yurun Feng*c, Xue Guoc, Yu Liuc and Hongyu Gong*c
aState Key Laboratory for Hydraulic Engineering Simulation and Safety, Tianjin University, Tianjin 250061, P. R. China
bSchool of Civil Engineering, Shandong University, Jinan 250061, P. R. China
cKey Laboratory for Liquid–Solid Evolution & Processing of Materials of Ministry of Education, Shandong University, Jinan 250061, P. R. China. E-mail: fengyurun@mail.sdu.edu.cn; hygong@sdu.edu.cn

Received 24th August 2017 , Accepted 25th September 2017

First published on 28th September 2017


Abstract

Fe-doped polymer-derived SiCN ceramics were synthesized by a precursor conversion method with different contents of nano-Fe2O3. The phase composition and microstructure were characterized by XRD, SEM and TEM. The results revealed that α-Fe and graphite phases were generated during the synthetic process. The electromagnetic and wave absorbing properties of the Fe-doped SiCN ceramics were analyzed with different amounts of nano-F2O3 over the frequency range of 2–18 GHz. The existence of α-Fe and graphite phases improved the electromagnetic properties of the materials greatly. The reflectance and electromagnetic attenuation coefficient of Fe-doped SiCN ceramics (15 wt% F2O3) reached −11 dB and 325 at 10.5 GHz, respectively, which indicated that the Fe-doped SiCN ceramics possessed excellent absorbing properties.


1. Introduction

With the rapid development of information technology, the interference between different sources of electromagnetic waves always leads to a decrease in the accuracy of data transmission and can even lead to the failure of the electronic device. Therefore, technology that effectively shields or absorbs electromagnetic waves is urgently needed. Although electromagnetic shielding materials are helpful to block the electromagnetic interference, they are incapable of weakening the electromagnetic wave fundamentally. However, the electromagnetic wave absorption materials can convert the energy of the electromagnetic wave into other forms, such as mechanical energy, thermal energy and power energy, thereby almost eliminating the influence of the electromagnetic wave.1,2 Traditional absorbing materials such as ferrite, the metal alloy, carbide ceramics, carbon-based materials, etc. present good absorbing intensity, but narrow absorption bands, ease of oxidation and high density limit their development.

Recently, polymer derived SiCN ceramics have attracted many interests due to the unique microstructures with carbon nano-domains,3 excellent thermal stability,4 oxidation and creep resistance5–7 and outstanding electric conductivity,8 which make them popular in applications of anode materials in lithium battery9,10 and high-temperature sensing devices.11 However, few researches put emphasis on the dielectric and microwave absorption properties of SiCN ceramics. Actually the SiCN ceramics have excellent dielectric properties in X-band.12 Additionally, the incorporation of magnetic materials (metallic fillers, such as Fe and its compounds) may offer new magnetic capabilities and microwave absorbing properties for the SiCN ceramics. Ralf Hauser et al.13 discussed the influence of Fe and Co addition on the magnetization of metal-containing SiCN ceramics. The metallic SiCN ceramics exhibit outstanding ferromagnetic behavior, indicating that the existence of magnetic materials could improve the dielectric properties and magnetic performance greatly.

In this work, the polymer-derived SiCN ceramics were synthesized by precursor conversion method with nano-Fe2O3 as magnetic filler. The effect of nano-Fe2O3 (6 wt%, 12 wt%, 15 wt%, 18 wt%) on the phase composition, microstructure and electromagnetic properties of the Fe-doped SiCN ceramics were analyzed.

2. Material and methods

Polysilazane (HTT1800, Haiyi Technology and Trading Co. Ltd., Shanghai) was used as the precursor. Dicumyl peroxide (DCP, 99%, Aladdin) was used as cross linking agent. The nano-Fe2O3 (D50 = 20 nm, α-Si3N4 > 93%, Beiing Tsinghua Unisplend or Founder High-Tech Ceramics Co. Ltd.) was added as magnetic filler. The HTT1800 and DCP were mixed at 70 °C and crosslinked at 600 °C under nitrogen flow atmosphere. After crushing and ball milling, the precrosslinked powder was uniformly mixed with different amounts of nano-Fe2O3 (6 wt%, 12 wt%, 15 wt% and 18 wt%). The mixed powders were pressed into green compacts and sintered at 1100 °C for 2 h under N2 atmosphere.

The phase compositions of samples were analyzed by the X-ray diffraction (XRD, X'pert Pro MPD, Japan). The microstructure characterization of SiCN ceramics was performed using SEM equipped with EDS (SU-70, Hitachi Co., Japan) and TEM (JEM-1200EX). The low-frequency permittivity of samples was identified by LCR digital electric bridge (TH2826, Changzhou Tonghui Electronic Co., Ltd). The permittivity and permeability of samples at frequency range of 2–18 GHz were analyzed by coaxial transmission reflection method through vector network analyzer (VNA, N 5244A, Agilent, USA). The sample was crushed and ground into fine powders, and then prepared into Φ7Φ3 coaxial rings with 2 mm thickness. The reflectance (R) and electromagnetic attenuation coefficient (α) were calculated by the following equations:

image file: c7ra09399c-t1.tif

image file: c7ra09399c-t2.tif

image file: c7ra09399c-t3.tif
where Zin was input impedance, εr was the permittivity, μr is the relative permeability, ε′ was the real part of permittivity, ε′′ was the imaginary part of permittivity, μ′ was the real permeability, μ′ was the imaginary permeability, f was the frequency of electromagnetic wave, c was the speed of light and d was the thickness of samples.

3. Results and discussion

Fig. 1 shows the XRD patterns of Fe-doped SiCN ceramics with different contents of nano-Fe2O3 powders. The sample exhibited amorphous diffraction peaks, and the main crystalline phases were α-Fe, and graphite. Additionally, the intensity of above peaks increased with the rising amount of nano-Fe2O3. The transformation of nano-Fe2O3 to α-Fe could be attributed to the formation of inner reductive atmosphere of hydrocarbons and hydrogen (CxHy, H2) during the pyrolysis process.14–16 According to the Scherrer equation,17 the size of α-Fe crystallites and graphite could be calculated to be about 35 nm and 20 nm, indicating the simultaneous formation of α-Fe and graphite crystallite in the Fe-doped SiCN ceramics.
image file: c7ra09399c-f1.tif
Fig. 1 XRD patterns of Fe-doped SiCN ceramics with different contents of nano-Fe2O3 (a) 6 wt%; (b) 12 wt%; (c) 15 wt%; (d) 18 wt%.

Fig. 2 represents the SEM micrographs of Fe-doped SiCN ceramics with different contents of nano-Fe2O3. It showed typical amorphous structure and large amounts of pores existed, meanwhile some minor second phase grain existed in the gap of large particles. The pores might be generated by the structural rearrangement and gas evolution process during the precursor conversion transformation. EDS was applied to analysis the element composition of the particle in the large particles and the grains in the gap.


image file: c7ra09399c-f2.tif
Fig. 2 SEM micrographs of Fe-doped SiCN ceramics with different contents of nano-Fe2O3 (a) 6 wt%; (b) 12 wt%; (c) 15 wt%.

The EDS spectra of Fe-doped SiCN ceramics with 12 wt% nano-Fe2O3 (Fig. 2(b) 1 and 2) were shown in Fig. 3. According to the elemental analysis, the main elements in the large particles (Fig. 2(b) area 1) were Si, C, N, indicating that the large particles were consisted of SiCN network frame structure. And the Fe element was hard to be detected in this area. However, the Fe elements (14.75%) and C elements could be easily detected in the second phase grains (Fig. 2(b) area 2), which was consistent with the XRD investigations where α-Fe was found as the main crystalline phase. Therefore, the α-Fe and graphite mainly concentrated in the gaps of large particles.


image file: c7ra09399c-f3.tif
Fig. 3 EDS spectra of Fe-doped SiCN ceramics with 12 wt% nano-Fe2O3 (panels 1 and 2 stand for EDS spectra of portions 1 and 2 in Fig. 2b).

Fig. 4 shows the HRTEM micrographs (a) and electron diffraction pattern (b) of Fe-doped SiCN ceramics with 15 wt% nano-Fe2O3. The grain size of spherical crystallites (Fig. 4(a)) was about 30 nm. Combined with the XRD analysis above, the spherical crystallites might be α-Fe. The electron diffraction pattern and parameters of the Fe-doped SiCN ceramics were shown in Fig. 4(b) and Table 1, respectively. The polycrystalline diffraction phenomenon of the sample, indicated the existence of several crystallites, such as α-Fe and graphite crystallites. As shown in the diffraction pattern parameters, the main crystal lattice structure (N = 2[thin space (1/6-em)]:[thin space (1/6-em)]4[thin space (1/6-em)]:[thin space (1/6-em)]6) belonged to body-centered cubic. In addition, the lattice constant (a) calculated in this study was about 2.850 Å, which was close to the standard lattice constant (2.866 Å) of α-Fe, suggesting the generation of α-Fe in the Fe-doped SiCN ceramics.


image file: c7ra09399c-f4.tif
Fig. 4 HRTEM micrographs (a) and electron diffraction pattern (b) of Fe-doped SiCN ceramics with 15 wt% nano-Fe2O3.
Table 1 Electron diffraction pattern parameters of Fe-doped SiCN ceramics with 15 wt% nano-Fe2O3
Diffractions circle 1 2 3
R (nm−1) 4.94 (R1) 7.07 (R2) 8.57 (R3)
Rj2/R12 1 2.04 3.01
N 2 4 6
{hkl} 110 200 112
d (Å) 2.02 1.41 1.17
a (Å) 2.862 2.829 2.858


Fig. 5 shows the dielectric constants of Fe-doped SiCN ceramics with different contents of nano-Fe2O3 at 1–5 MHz. Under the same frequency, the appearance of graphite phase particles acting as carriers like space charges and dipoles, resulted in growth of the dielectric constant of Fe-doped SiCN ceramics with the rising amount of nano-Fe2O3 basically.


image file: c7ra09399c-f5.tif
Fig. 5 Dielectric constants of Fe-doped SiCN ceramics with different contents of nano-Fe2O3.

The dielectric properties of Fe-doped SiCN ceramics with different contents of nano-Fe2O3 at the microwave frequency (2–18 GHz) are shown in Fig. 6. The real part of dielectric constant increased with the rising percentage of nano-Fe2O3 (Fig. 6(a)). The values of imaginary permittivity (Fig. 6(b)) and the loss tangent (Fig. 6(c)) were both indistinguishable for all samples except that sample with 15 and 18 wt% nano-Fe2O3. The resonance peak at 9.5 GHz depended on the change in polarization mechanism of dielectric materials including displacement polarization and turning-direction polarization.18 The maximum value of imaginary permittivity and loss tangent of the Fe-doped SiCN ceramics with 15 wt% nano-Fe2O3 were 0.65 and 0.13, respectively. Meanwhile, the increasing of dielectric loss had strengthened the wave absorbing properties.


image file: c7ra09399c-f6.tif
Fig. 6 The dielectric properties of Fe-doped SiCN ceramics with different contents of nano-Fe2O3 (a) real permittivity; (b) imaginary permittivity; (c) dielectric loss angle tangent.

The magnetic properties of Fe-doped SiCN ceramics with different contents of nano-Fe2O3 at the microwave frequency (2–18 GHz) are shown in Fig. 7. The real permeability (Fig. 7(a)) confirmed the ferromagnetic characteristics of the Fe-doped SiCN ceramics. The imaginary permeability (Fig. 7(b)) and magnetic loss angle tangent (Fig. 7(c)) of resonance peaks 12 wt% and 15 wt% nano-Fe2O3 emerged around 10.5 GHz, which might be caused by the existence of ferromagnetic resonance by α-Fe phase. The maximum values of imaginary permittivity and magnetic loss angle tangent of the Fe-doped SiCN ceramics with 15 wt% nano-Fe2O3 were 1.58 and 6.5, respectively.


image file: c7ra09399c-f7.tif
Fig. 7 The magnetic properties of Fe-doped SiCN ceramics with different contents of nano-Fe2O3 (a) real permeability; (b) imaginary permeability; (c) magnetic loss angle tangent.

The dielectric properties and magnetic properties of Fe-doped SiCN ceramics changed obviously when samples with 15 wt% nano-Fe2O3. Fig. 8 shows the relationship between dielectric parameters (real part and imaginary part) and frequency of Fe-doped SiCN ceramics (15 wt% nano-Fe2O3). The damping harmonic oscillator relaxation of the sample might lead to the resonance peak in 8–12 GHz. It might be caused by the displacement polarization withdrawal of negative and positive ions in the free carbon.


image file: c7ra09399c-f8.tif
Fig. 8 The real part and imaginary part of Fe-doped SiCN ceramics (15 wt% nano-Fe2O3) with different frequency.

The wave absorbing performance depended on the dielectric and magnetic properties. Fig. 9 shows the reflectance (R) and electromagnetic attenuation coefficient (α) of Fe-doped SiCN ceramics (thickness 2 mm) at 2–18 GHz. The value of R decreased with the increasing of frequency except the samples with 15 wt% and 18 wt% nano-Fe2O3 around 10 GHz. Similarity, the resonance peaks of α-Fe were formed in the same frequency. The phenomenon above might be related to the superposition effect of dielectric loss and magnetic loss. The minimum value of reflectance for Fe-doped SiCN ceramics with 15 wt% nano-Fe2O3 was −11 dB at 10.5 GHz and electromagnetic attenuation coefficient reached up to 325 in the same frequency, which indicated that the Fe-doped SiCN ceramics possessed excellent wave absorbing properties.


image file: c7ra09399c-f9.tif
Fig. 9 The wave absorbing properties of Fe-doped SiCN ceramics with different contents of nano-Fe2O3 (a) reflectance; (b) electromagnetic attenuation coefficient.

Table 2 shows the comparison of wave absorbing properties of Fe-doped SiCN ceramics with other composites from the literature. The reflectance of the samples was similar, but the synthesized temperature in this study was much lower than other references. Therefore, the application of Fe-doped SiCN ceramics could greatly reduce the production cost and possess potential prospect in wave adsorbing materials.

Table 2 Comparison of wave absorbing properties of Fe-doped SiCN ceramics with other composites from the literature
Samples Reflectance in X-band (dB) Thickness (mm) Tem. (°C) Ref.
Fe-doped SiCN −11 2 1100 This work
PDCs-SiBCN −15.78 2.31 1650 18
PDCs-SiBCN −13.35 2.18 1800 18
PDCs-SiCN −18 2 1700 19


4. Conclusions

The Fe-doped polymer-derived SiCN ceramics were synthesized by precursor conversion method with different content of nano-Fe2O3. The α-Fe and graphite phases were generated during the synthetic process. The existence of α-Fe and graphite phases could improve the electromagnetic and wave absorbing properties of the Fe-doped polymer-derived SiCN ceramics greatly. The reflectance and electromagnetic attenuation coefficient of Fe-doped SiCN ceramics with 15 wt% nano-Fe2O3 were −11 dB and 325 at 10.5 GHz, illustrating that the Fe-doped SiCN ceramics possessed excellent wave absorbing properties.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This work was financially supported by the National Natural Science Foundation of China (No. 51572154) and Shandong Nature Science Foundation of China (2015ZRE27348).

References

  1. D. D. L. Chung, Electromagnetic interference shielding effectiveness of carbon materials, Carbon, 2001, 39(2), 279–285 CrossRef CAS.
  2. L. Kong, X. Yin and F. Ye, et al., Electromagnetic wave absorption properties of ZnO-based materials modified with ZnAl2O4 nanograins, J. Phys. Chem. C, 2013, 117(5), 2135–2146 CAS.
  3. S. Widgeon, G. Mera and Y. Gao, et al., Nanostructure and energetics of carbon-rich SiCN ceramics derived from polysilyl carbodiimides: role of the nanodomain interfaces, Chem. Mater., 2012, 24(6), 1181–1191 CrossRef CAS.
  4. R. Riedel, A. Kienzle and W. Dressler, et al., A silicoboron carbonitride ceramic stable to 2000 °C, Nature, 1996, 382(6594), 796–798 CrossRef CAS.
  5. Y. Wang, Y. Fan and L. Zhang, et al., Polymer-derived SiAlCN ceramics resist oxidation at 1400 °C, Scr. Mater., 2006, 55(4), 295–297 CrossRef CAS.
  6. Y. Wang, W. Fei and Y. Fan, et al., Silicoaluminum carbonitride ceramic resist to oxidation/corrosion in water vapor, J. Mater. Res., 2006, 21(07), 1625–1628 CrossRef CAS.
  7. R. Riedel, L. M. Ruwisch and L. An, et al., Amorphous silicoboron carbonitride ceramic with very high viscosity at ultra high temperatures, J. Am. Ceram. Soc., 1998, 81, 3341–3344 CrossRef CAS.
  8. X. Li, K. Wang and B. Ma, et al., Effect of acrylic acid additive on electric conductivity of polymer-derived amorphous silicon carbonitride, Ceram. Int., 2015, 41(6), 7971–7976 CrossRef CAS.
  9. M. Wilamowska, M. Graczyk-Zajac and R. Riedel, Composite materials based on polymer-derived SiCN ceramic and disordered hard carbons as anodes for lithium-ion batteries, J. Power Sources, 2013, 244, 80–86 CrossRef CAS.
  10. L. M. Reinold, Y. Yamada and M. Graczyk-Zajac, et al., The influence of the pyrolysis temperature on the electrochemical behavior of carbon-rich SiCN polymer-derived ceramics as anode materials in lithium-ion batteries, J. Power Sources, 2015, 282, 409–415 CrossRef CAS.
  11. X. Ren, S. Ebadi and Y. Chen, et al., Characterization of SiCN ceramic material dielectric properties at high temperatures for harsh environment sensing applications, IEEE Trans. Microwave Theory Tech., 2013, 61(2), 960–971 CrossRef CAS.
  12. Q. Li, X. Yin and L. Feng, Dielectric properties of Si3N4-SiCN composite ceramics in X-band, Ceram. Int., 2012, 38(7), 6015–6020 CrossRef CAS.
  13. R. Hauser, A. Francis and R. Theismann, et al., Processing and magnetic properties of metal-containing SiCN ceramic micro- and nano-composites, J. Mater. Sci., 2008, 43(12), 4042–4049 CrossRef CAS.
  14. M. Malenovska, S. Martinez and M. A. Neouze, et al., Growth of Metal Nanoparticles in a Sol-Gel Silica Thin Film, Eur. J. Inorg. Chem., 2007, 18, 2609–2611 CrossRef.
  15. V. S. Gurin, V. P. Petranovskii and N. E. Bogdanchikova, Metal clusters and nano particles assembled in zeolites: an example of stable materials with controllable particle size, Mater. Sci. Eng., C, 2002, 19(1), 327–331 CrossRef.
  16. L. Kim, E. Lee and S. J. Cho, et al., Diameter control of carbon nanotubes by changing the concentration of catalytic metal ion solutions, Carbon, 2005, 43(7), 1453–1459 CrossRef CAS.
  17. H. Sun, Y. Zhang and H. Gong, et al., High Reactive MgO-Y2O3 Nanopowders Via Microwave Combustion Method and Sintering Behavior, Int. J. Appl. Ceram. Technol., 2016, 13(2), 367–372 CrossRef CAS.
  18. F. Ye, L. Zhang and X. Yin, et al., Dielectric and EMW absorbing properties of PDCs-SiBCN annealed at different temperatures, J. Eur. Ceram. Soc., 2013, 33(8), 1469–1477 CrossRef CAS.
  19. Q. Li, X. Yin, W. Duan, B. Hao, L. Kong and X. Liu, Dielectric and microwave absorption properties of polymer derived SiCN ceramics annealed in N2 atmosphere, J. Eur. Ceram. Soc., 2014, 34, 589–598 CrossRef CAS.

This journal is © The Royal Society of Chemistry 2017