Open Access Article
This Open Access Article is licensed under a Creative Commons Attribution-Non Commercial 3.0 Unported Licence

Pebax-based composite membranes with high gas transport properties enhanced by ionic liquids for CO2 separation

Mengdie Liab, Xiangping Zhang*a, Shaojuan Zenga, Lu baia, Hongshuai Gaoa, Jing Dengab, Qingyuan Yangc and Suojiang Zhang*a
aBeijing Key Laboratory of Ionic Liquids Clean Process, State Key Laboratory of Multiphase Complex Systems, Beijing Key Laboratory of Ionic Liquids Clean Process, Institute of Process Engineering, Chinese Academy of Sciences, Beijing 100190, China. E-mail: xpzhang@ipe.ac.cn; sjzhang@ipe.ac.cn
bSchool of Chemistry and Chemical Engineering, University of Chinese Academy of Sciences, Beijing 100049, China
cState Key Laboratory of Organic–Inorganic Composites, Beijing University of Chemical Technology, Beijing 100029, China

Received 23rd November 2016 , Accepted 29th December 2016

First published on 19th January 2017


Abstract

Membrane-based separation technology has been reported as one of the possible methods to efficiently and economically separate carbon dioxide (CO2). To provide synergistic enhancements in the gas separation performance, organic polymer (Pebax 1657), zeolite imidazolate framework-8 (ZIF-8) nanoparticles, and ionic liquid (IL) have been integrated to develop three-component composite membranes. To achieve high separation performance of three-component membranes, the effects of IL anions and ZIF-8 content on gas permeability and selectivity were investigated first. The ILs were 1-butyl-3-methyl imidazolium ([Bmim]) cation based on different anions of bis(trifluoromethylsulfonyl)imide ([NTf2]), dicyanamide ([DCA]), and tetrafluoroborate ([BF4]). Gas transport properties of all the prepared membranes were investigated at 23 °C and 1 bar. The results showed that the anion of IL is a key factor to determine the CO2 permeability of the membranes, which is similar to the principle of CO2 solubility in pure ILs. In addition, ZIF-8 could increase both CO2 diffusivity and solubility coefficients of the Pebax/ZIF-8 membranes, resulting in a two-fold increase in the CO2 permeability. For the Pebax/ZIF-8(15%)/[Bmim][NTf2] membranes, it has been revealed that [Bmim][NTf2] acts as a low molecular weight additive, leading to a more amorphous structure and a higher FFV (fractional free volume) of the membranes, which are beneficial for gas diffusion. The addition of IL can improve the compatibility between the inorganic particles and the polymer matrix; thus, the non-selective voids decrease, which leads to a higher CO2/N2 selectivity. The CO2 permeability of the Pebax/ZIF-8(15%)/IL(80%) membrane was 4.3 times that of the pure Pebax membrane without sacrificing the CO2/N2 selectivity. Therefore, the high gas transport properties of the Pebax/ZIF-8/IL membranes make them promising candidates for CO2-effective separation materials.


1. Introduction

Owing to global warming and increasing energy consumption, the efficient separation of CO2 has received significant interest.1,2 During the last few decades, various methods have been developed for CO2 separation. Compared to the traditional methods, such as solvent absorption, pressure- and temperature-swing adsorption, and cryogenic distillation, the membrane method has become an emerging technology because of its advantages of environmentally friendliness, lower energy consumption, and ability for scale up.3,4 Owing to the good mechanical stability and easy processability, polymeric membranes have attracted considerable attention and have been studied in the separation of biogas (CO2/CH4),5,6 flue gas (CO2/N2),7,8 syngas (CO2/H2),9,10 and other light gases.11 However, there is a trade-off between permeability and selectivity known as the “Robeson upper-bound” that limits the application of polymeric membranes for gas separation.

Hence, due to the difficulty in achieving a simultaneously high gas permeability and selectivity for a single polymer material, mixed-matrix membranes (MMMs), which are a blend of organic polymers and inorganic materials, offer an opportunity to overcome the trade-off limit.12–14 Inorganic materials, such as molecular sieves, carbon nanotubes, mesoporous materials, zeolites, and metal–organic frameworks, provide high gas flux and selectivity as well as good thermal and chemical stability in MMMs.13 However, challenges are encountered with the interfacial defects and poor adhesion between inorganic particles and polymer matrix.13

Ionic liquids (ILs) have been regarded as attractive absorbents of CO2 owing to their high CO2 absorption capacity, low volatility, and tunable characteristics.15 Some ILs, which have the cations, such as imidazolium, ammonium, phosphonium, pyridinium, and pyrrolidinium, and anions, such as bis(trifluoromethylsulfonyl)imide ([NTf2]), tetrafluoroborate ([BF4]), and dicyanamide ([DCA]), have been extensively used in CO2 absorption.16 Moreover, recent studies have shown that IL as an additive can enhance the interfacial adhesion between the polymer matrix and inorganic particles, as well as the CO2 adsorption.17,18 Mohshim's et al.19 found that incorporating [Emim][NTf2] (1-ethyl-3-methyl imidazolium bis(trifluoromethylsulfonyl)imide) into PES (polyethersulfone)-SAPO-34 MMMs could reduce the agglomeration of the filler particles and produce defect-free mixed matrix membranes. Therefore, combining ILs with MMMs would offer an opportunity to improve the compatibility between the inorganic particles and polymer matrix as well as achieve good dispersion. Furthermore, IL-based membranes may be considered as an approach to avoid the lower diffusivity and flux caused by the high viscosities of ILs.

In this study, to achieve synergistic enhancements in the gas separation performance, organic polymer (Pebax 1657), zeolite imidazolate framework-8 (ZIF-8) nanoparticles, and ionic liquid (IL) were integrated to develop three-component membranes. Poly(ether-b-amide-6) (Pebax 1657) was selected as the polymer matrix because of its easy film formation, economical feasibility, and relatively high CO2 separation performance. The soft PEO segments in Pebax can act as a permeable phase because of its high chain mobility and high affinity of the EO unit for the CO2 molecule. In addition, the hard PA segments in Pebax can impart mechanical stability to the polymer.20,21 Zeolite imidazolate framework-8 (ZIF-8) was chosen as the inorganic filler because it has certain selectivity towards CO2 and is widely used in CO2/CH4, CO2/N2 separation.22,23 [Bmim] cation-based ILs were selected because the imidazolium group tends to have excellent CO2 solubility.24

For better preparation of the three-component composite membranes, Pebax/IL membranes composed of three types of anion, [NTf2], [DCA], and [BF4], and Pebax/ZIF-8 composite membranes with a ZIF-8 content varying from 0–20 wt% have been firstly studied. The chemical structures of Pebax 1657 and ILs used in this study are shown in Fig. 1. The membranes prepared in this study were characterized by FTIR (Fourier transform infrared spectroscopy), XRD (X-ray diffraction), and SEM (scanning electron microscopy). The thermal properties were measured by DSC (differential scanning calorimetry) and TGA (thermogravimetric analysis). The gas permeability (P), selectivity (α), diffusivity coefficients (D), and solubility coefficients (S) of the membranes were systematically studied at 23 °C and 1 bar.


image file: c6ra27221e-f1.tif
Fig. 1 Chemical structures of (a) Pebax 1657, (b) [Bmim][NTf2], (c) [Bmim][BF4], and (d) [Bmim][DCA].

2. Experimental

2.1 Materials

Pebax 1657 (containing 60% PEO and 40% PA) was provided by Shanghai Connell Bros. Company. ZIF-8 was purchased from Sigma-Aldrich. [Bmim][NTf2], [Bmim][DCA], and [Bmim][BF4] were supplied by the Linzhou Keneng Materials Technology Co., Ltd. Ethanol was purchased from Beijing Chemical Works, and deionized water was used throughout the study. The gases (CO2 99.99%, CH4 99.99%, and N2 99.99%) used in the permeation experiment were supplied by Beijing Beiwen Gas Factory.

2.2 Preparation of membranes

2.2.1 Pebax/IL and Pebax/ZIF-8 composite membranes. Pebax solution (8 wt%) was prepared by dissolving the Pebax pellets in a mixture of ethanol/water (70/30 depending on weight) at 80 °C under reflux and vigorous stirring for at least 8 h. After cooling the Pebax solution down to ambient temperature, a certain amount of IL or ZIF-8 particles were slowly added to the Pebax solution. In this study, the content was based on the weight of the polymer Pebax 1657. To avoid the agglomeration of ZIF-8, the solution was ultrasonicated for at least 3 h and stirred for 10 min after 30 min ultrasonication. After stirring overnight under ambient conditions, the homogeneous solution was cast onto a square glass plate and dried under ambient conditions for 24 h. Finally, all the membranes were dried in a vacuum oven at 50 °C for two days to remove the residual solvent.
2.2.2 Pebax/ZIF-8/IL three-component composite membranes. The three-composite membranes were prepared following a similar abovementioned procedure. In a typical experiment, a certain amount of IL was first added to the Pebax solution and completely dissolved during 2 h stirring. Then, ZIF-8 particles were added to the solution and stirred for another 24 h. Finally, the homogeneous solution was cast onto a square glass plate and dried in a vacuum oven to remove the solvent.

2.3 Characterization of the membranes

The FTIR spectra were obtained by a Thermo Nicolet 380 spectrometer in the range of 750–4000 cm−1 under ambient conditions. The thermal properties of the membranes were investigated over the temperature range from −100 °C to 250 °C at a heating rate of 10 °C min−1 under N2 atmosphere by Mettler-Toledo DSC1. DTG-60H was used to determine the weight changes as a function of temperature over time in a N2 controlled atmosphere at 10 °C min−1 from 50 °C to 550 °C. XRD patterns of the prepared membranes were obtained using a Smartlab (9 kW) from 5 to 60° 2θ values at a rate of 10° min−1. Scanning electron microscopy was performed using a SU8020 to analyze the morphological structure of the composite membranes. Before scanning, the samples required to be fractured in liquid nitrogen, and then coated with gold.

2.4 Gas permeation experiments

Gas permeability tester (VAC-V2, Labthink) was used to examine the pure gas permeation of these prepared membranes with the constant volume/variable pressure method. All the test gases were proceeded in the order of N2, CH4, and CO2 at 23 °C and 1 bar. Before each test, the permeate side of the membrane was evacuated. The gas permeability (P), diffusion coefficient (D), solution coefficient (S), and ideal selectivity (αA/B) of the membranes were calculated using the following equations:
 
image file: c6ra27221e-t1.tif(1)
where P represents the gas permeability [barrer, 1 barrer = 10−10 cm3(STP) per cm per (cm2 s cm Hg)] and A stands for the area of the membrane (cm2). The active membrane area for the gas permeation measurements in this experiment was 4.9 cm2. V means the downstream volume (cm3), T is the operating temperature (K), d represents the membrane thickness (cm), and the thickness of the prepared membranes for the permeability measurement is listed in Table S1. (p1p2) means the transmembrane pressure difference (cm Hg), Δpt, is the arithmetic average of the gas pressure changes in the low pressure chamber in unit time when the gas stably permeates through the membrane, T0 and P0 means the temperature (273.15 K) and pressure (1.0133 × 105 Pa) under standard conditions.

D is the diffusion coefficient (cm2 s−1), which can be determined by the time-lag (θ) method.

 
image file: c6ra27221e-t2.tif(2)

Based on the solution-diffusion mechanism, the solubility coefficients (S) can be obtained from eqn (3):

 
image file: c6ra27221e-t3.tif(3)

The ideal selectivity αA/B can be calculated from eqn (4):

 
image file: c6ra27221e-t4.tif(4)

3. Results and discussion

3.1 Characterization of the membranes

3.1.1 Fourier transform infrared (FTIR) spectroscopy. The interaction between Pebax 1657, ZIF-8, and IL can be investigated from the FTIR spectra, as shown in Fig. 2. For the pure Pebax membranes, the characteristic peaks at around 1102, 1733, and 2867 cm−1 are the stretching vibrations of C–O, C[double bond, length as m-dash]O, and –CH3, respectively. The peaks at 1638 and 3300 cm−1 were assigned to the H–N–C[double bond, length as m-dash]O and N–H group, respectively.25 The bands for ZIF-8 at 1580 cm−1 and 1145, 990 cm−1 correspond to the C[double bond, length as m-dash]N and C–N stretching, respectively.26 Several FTIR peaks corresponding to [Bmim][NTf2], 1055 cm−1 (S[double bond, length as m-dash]O bending), 1431 cm−1 (C[double bond, length as m-dash]C stretching), 1575 cm−1 (C[double bond, length as m-dash]N stretching), and 1250–1150 cm−1 (C–F stretching), 3000–2900 cm−1 (C–H stretching), and 3200–3000 cm−1 (ring C–H stretching) were observed.27 In addition, the spectra of the pure IL, ZIF-8, and Pebax showed no new peaks for all the composite membranes, implying the physical blending feature of ZIF-8 and [Bmim][NTf2] within the Pebax bulk.
image file: c6ra27221e-f2.tif
Fig. 2 FTIR spectra of (a) Pebax, (b) ZIF-8, (c) Pebax-ZIF-8(15%), (d) [Bmim][NTf2], and (e) Pebax-ZIF-8(15%)-IL(20%) composite membranes.
3.1.2 X-ray diffraction (XRD). XRD patterns of Pebax, ZIF-8, and Pebax composite membranes were obtained to further investigate their nanostructures (Fig. 3). The pure Pebax is a semicrystalline copolymer containing a crystalline phase (PA) and an amorphous phase (PEO), with diffraction peaks at 13.70, 16.52, 23.68, and 25.10° (2θ), and the peaks at 23.70° and 25.16° result from the crystalline PA and PEO phase, respectively.25,28 For pure ZIF-8, there are diffraction peaks at 2θ = 7.26, 10.32, 12.66, 14.64, 16.38, and 17.96° for the {110}, {200}, {211}, {220}, {310}, and {222} planes, respectively.29 When the ZIF-8 content reached 15 wt%, there were characteristic peaks of ZIF-8 arising in the spectra of Pebax/ZIF-8 composite membranes. The addition of IL and ZIF-8 slightly decreased the d-spacing of the diffraction peak at 23.70°, indicating that the inter-chain hydrogen bonding between PA segments in Pebax is disturbed and amorphous region increases within the membranes.30
image file: c6ra27221e-f3.tif
Fig. 3 XRD patterns of Pebax, ZIF-8, and Pebax composite membranes.
3.1.3 Thermal properties of the prepared membranes. The thermal properties of IL, ZIF-8, Pebax, and Pebax composite membranes were investigated by differential scanning calorimetry (DSC) and thermogravimetric analysis (TGA). The DSC curves of Pebax and Pebax composite membranes are shown in Fig. S1 and the glass transition temperatures (Tg) are listed in Table 1. The results show that Tg of Pebax/ZIF-8 membranes increases with the increasing ZIF-8 content due to polymer chain rigidification caused by the interactions between ZIF-8 and Pebax polymer.31 However, Tg of the Pebax/ZIF-8/IL membranes decreases with the increasing IL content, implying a higher chain mobility of the polymer matrix.32 For the pure Pebax membrane, two characteristic melting peaks were observed at around 19 and 206 °C, which were assigned to the melting point of PEO crystals and PA crystallites. With the addition of ZIF-8 and IL, the melting peaks of PA segment for all Pebax-based membranes were shifted to a lower temperature, resulting from the reduction in the crystallinity and increase in the chain mobility. In addition, the melting peaks of PEO become weaker with the addition of IL and even disappear after 30 wt% IL content. This is due to the decrease in the PEO crystallinity and the miscibility of PEO and IL.33
Table 1 Physical properties of the ZIF-8, IL, Pebax, and Pebax composite membranes
Membrane Tda (°C) Tgb (°C) ΔHm (J g−1) Xcrystallinityc (%)
PEO PA PEO PA Total
a Decomposition temperature of the prepared membranes, ZIF-8, and [Bmim][NTf2].b Glass transition temperature of the prepared membranes and [Bmim][NTf2].c Total crystallinity of the prepared membranes.
Pebax 363.86 −50.48 24.12 28.29 14.50 12.30 13.62
Pebax-ZIF(5%) 334.01 −49.45 23.49 24.76 14.12 10.77 12.78
Pebax-ZIF(15%) 335.76 −47.31 19.78 21.25 11.89 9.24 10.83
Pebax-ZIF(15%)-IL(5%) 336.37 −48.86 17.62 21.02 10.59 9.14 10.01
Pebax-ZIF(15%)-IL(15%) 331.32 −50.71 9.72 19.22 5.84 8.36 6.85
Pebax-ZIF(15%)-IL(20%) 331.60 −52.99 5.83 17.98 3.50 7.82 5.23
Pebax-ZIF(15%)-IL(30%) 330.52 −53.43 16.42 7.14 2.86
Pebax-ZIF(15%)-IL(40%) 331.37 −54.05 15.52 6.75 2.70
Pebax-ZIF(15%)-IL(60%) 333.56 −55.71 13.29 5.78 2.31
Pebax-ZIF(15%)-IL(80%) 336.22 −57.78 10.14 4.41 1.76
ZIF-8 495.94
[Bmim][NTf2] 380.70 −96.37


Furthermore, the crystallinity of the prepared membranes was calculated using the DSC thermograms according to eqn (5):

 
image file: c6ra27221e-t5.tif(5)
where ΔHm is the heat of melting of the crystals and can be calculated by integrating the area of the melting peaks, ΔH0m represents the heat of melting as if the polymer is 100% crystalline. ΔH0m of PEO (166.4 J g−1) and PA (230.0 J g−1) were obtained from the literature.34 The total crystallinity (Xcrystallinity) of the prepared membranes was calculated by considering 40% PA crystallinity and 60% PEO crystallinity.32 The calculation results are also listed in Table 1. Both ZIF-8 and IL decrease the total crystallinity of the prepared membranes, leading to a greater chain mobility and higher fractional free volume (FFV) of the membranes, which are beneficial for gas diffusion.35

In addition, the thermal stabilities of the membranes were also studied by thermogravimetric analysis (TGA). The TGA curves of ZIF-8, [Bmim][NTf2], and prepared membranes are shown in Fig. S2. The decomposition temperatures (Td) at 5% weight loss are listed in Table 1. The results show that Td of the Pebax 1657 membrane, IL, and ZIF-8 is 363.86, 380.70, and 495.94 °C, respectively. The addition of ZIF-8 decreases the Td of the Pebax/ZIF-8 membranes compared to that of the pure Pebax membrane. However, the addition of IL does not significantly change the Td of the Pebax/ZIF-8/IL membranes compared to that of the Pebax/ZIF-8 membrane at 15 wt% ZIF-8. The Pebax/ZIF-8/IL membranes display two-step decomposition; the first step is around 360 °C based on Pebax and the second one is around 380 °C based on the IL. Overall, the Td of Pebax, Pebax/ZIF-8, and Pebax/ZIF-8/IL membranes was all above 330 °C, implying that all the prepared membranes have excellent thermal stability.

3.1.4 Scanning electron microscopy (SEM). SEM images of the surface and cross-sectional morphology of the prepared membranes are presented in Fig. 4 and 5, respectively. Fig. 4(a) and (b) show that pure Pebax membrane has a homogeneous, smooth surface, and the surface of the Pebax/ZIF-8 membranes becomes rougher with the addition of ZIF-8. Moreover, the ZIF-8 particles can be obviously observed in the cross-section of the Pebax/ZIF-8 membrane at 15 wt% ZIF-8 content, and a few microsized ZIF-8 agglomerates can be observed in Fig. 5(b). Compared to the Pebax/ZIF-8(15%) membrane, the surface of the Pebax/ZIF-8/IL membranes is smoother and the structure of the membranes becomes more amorphous with the increasing IL content. This may be attributed to the reduction in the crystallinity and is in accordance with the plasticization effects of the low-molecular weight additives reported in some studies.32,34 Fig. 5(c) and (d) show that IL decreases the interfacial voids between Pebax and ZIF-8. At 80 wt% IL content, and the amorphous morphology is quite clear, which will have a great impact on the diffusivity coefficients of the prepared membranes.
image file: c6ra27221e-f4.tif
Fig. 4 SEM images for the surface morphology of the prepared membranes. (a) Pure Pebax membrane, (b) Pebax-ZIF(15%) membrane, (c) Pebax-ZIF(15%)-IL(20%) membrane, and (d) Pebax-ZIF(15%)-IL(80%) membrane.

image file: c6ra27221e-f5.tif
Fig. 5 SEM images of the cross-section morphology of the prepared membranes. (a) Pure Pebax membrane, (b) Pebax-ZIF(15%) membrane, (c) Pebax-ZIF(15%)-IL(20%) membrane, and (d) Pebax-ZIF(15%)-IL(80%) membrane.

3.2 Gas separation performance of the Pebax/IL composite membranes

3.2.1 Effect of the IL anion on the gas permeability of the Pebax/IL composite membranes. The effect of the IL anion on the gas permeability of the Pebax/IL composite membranes was studied and is shown in Fig. 6. The permeability of N2, CH4, and CO2 for all the Pebax/IL membranes obviously increased compared to that for the pure Pebax membrane. For example, Pebax-[Bmim][BF4](100%), Pebax-[Bmim][DCA](100%), and Pebax-[Bmim][NTf2](100%) membranes exhibit higher CO2 permeability of 90.8, 126.4, and 157.3 barrer, respectively, vs. 53.70 barrer for the pure Pebax membrane. Moreover, CO2 permeability of the Pebax/IL membranes was in the following order: Pebax/[Bmim][NTf2] > Pebax/[Bmim][DCA] > Pebax/[Bmim][BF4]. It was demonstrated by some researchers that the anion plays a primary role in the CO2 solubility for the conventional ILs. The solubility of CO2 in the [Bmim]+-based ILs increases in the following order: [BF4] < [DCA] < [NTf2] at 25 °C, according to the Henry's law constants reported by Lei.15 It reveals that the anion is still a key factor to determine the CO2 permeability of the Pebax/IL membranes, which are familiar with the principle of CO2 in pure ILs. The gas permeability of N2 and CH4 follow the order Pebax/[Bmim][NTf2] > Pebax/[Bmim][BF4] > Pebax/[Bmim][DCA] and Pebax/[Bmim][NTf2] > Pebax/[Bmim][DCA] > Pebax/[Bmim][BF4], respectively.
image file: c6ra27221e-f6.tif
Fig. 6 Gas permeabilities of (a) CO2, (b) N2, and (c) CH4 for the Pebax/IL membranes as a function of IL content.
3.2.2 Effect of the IL anion on the gas selectivity of the Pebax/IL composite membranes. The CO2/N2 and CO2/CH4 selectivities of the Pebax/IL composite membranes are presented in Fig. 7. Compared to that of the pure Pebax membranes, the CO2/N2 selectivity of the Pebax/[Bmim][NTf2] and Pebax/[Bmim][BF4] composite membranes decreased, whereas that of the Pebax/[Bmim][DCA] membranes was nearly constant with the increasing IL content. For the Pebax/[Bmim][NTf2] and Pebax/[Bmim][DCA] membranes, there is a slight decrease in the CO2/CH4 selectivity. Furthermore, the selectivity of CO2/N2 and CO2/CH4 for the Pebax/IL composite membranes was in the following order: Pebax/[Bmim][DCA] > Pebax/[Bmim][NTf2] > Pebax/[Bmim][BF4] and Pebax/[Bmim][BF4] > Pebax/[Bmim][NTf2] > Pebax/[Bmim][DCA], respectively. This suggests that the selectivity of the Pebax/IL membranes depends on the affinity of the IL for the polymer and the inherent gas selectivity capacity of the ILs. Overall, [Bmim][NTf2] shows an optimal CO2 permeability and has been developed to prepare the three-component membranes in the following experiments. The mechanism of the effect of IL addition on gas separation performance has been discussed in Section 3.4.
image file: c6ra27221e-f7.tif
Fig. 7 Ideal selectivities of (a) CO2/N2 and (b) CO2/CH4 for the Pebax/IL membranes as a function of IL content.

3.3 Gas separation performance of the Pebax/ZIF-8 composite membranes

3.3.1 Effect of ZIF-8 addition on the gas diffusivity and solubility coefficients. Fig. 8 shows that the order of the diffusivity coefficients for the pure Pebax membrane is CH4 < N2 < CO2. For pure polymeric membranes, the diffusivity coefficients mainly depend on the kinetic diameter, based on the solution-diffusion model.25 Therefore, the experimental results are consistent with the theoretical results because the order of kinetic diameter is CH4 (0.38 nm) > N2 (0.36 nm) > CO2 (0.33 nm). The diffusivity coefficients of CO2 for the Pebax/ZIF-8 membranes increase with the ZIF-8 addition, owing to the reduction of polymer crystallinity, as shown in Fig. 4 and Table 1.30,36 Moreover, the agglomeration of ZIF-8 may produce narrow gaps or voids to facilitate gas diffusion, as observed in the SEM images. However, the diffusivity coefficients of N2 and CH4 showed an opposite trend. The cavity diameter of ZIF-8 was 0.34 nm, whereas the kinetic diameter of N2 and CH4 was 0.36 nm and 0.38 nm, respectively. Therefore, ZIF-8 favors the diffusion of CO2, whereas N2 and CH4 could not easily diffuse. Therefore, the diffusivity coefficients of N2 and CH4 decrease.
image file: c6ra27221e-f8.tif
Fig. 8 (a) Diffusivity coefficients and (b) solubility coefficients of N2, CH4, and CO2 for pure Pebax membranes and Pebax/ZIF-8 composite membranes as a function of ZIF-8 content.

Fig. 8(b) shows that the solubility coefficients of the Pebax/ZIF-8 composite membranes for all the gases increase with the addition of ZIF-8 due to the affinity between N2, CH4, and ZIF-8.37 In addition, CO2 has the highest solubility coefficients compared to those of N2 and CH4. The high solubility coefficients of CO2 are due to the high CO2 condensability and the quadrupole–dipole interaction between the CO2 molecules and EO units.35,38 In general, the gas permeability is determined by both diffusivity coefficients and solubility coefficients according to the solution-diffusion model (P = S × D).

3.3.2 Effect of ZIF-8 addition on the gas permeability and selectivity. Fig. 9 shows that the CO2 permeability of the Pebax/ZIF-8 membranes dramatically increases with the addition of ZIF-8, from 53.7 barrer to 124.6 barrer with the addition of ZIF-8 content from 0–20 wt%, which is approximately 132% higher than that of the pure Pebax membrane. The permeabilities of N2 and CH4 also increased by 128% and 165% compared to that of the pure Pebax membrane. The increase in the CO2 permeability is mainly due to the rapid gas diffusivity and high solubility with the addition of ZIF-8. The permeabilities of N2 and CH4 still increased, whereas the diffusivity coefficients decreased because of the significantly enhanced solubility coefficients. This suggests that gas transport in the Pebax/ZIF-8 membranes is more solubility-controlled, which is general for the rubbery polymer membranes.39
image file: c6ra27221e-f9.tif
Fig. 9 Gas permeability of N2, CH4, and CO2 for the pure Pebax membrane and Pebax/ZIF-8 membranes as a function of ZIF-8 content.

The selectivities of the pure Pebax membrane and Pebax/ZIF-8 membranes for CO2/N2 and CO2/CH4 are shown in Fig. 10. The addition of ZIF-8 slightly increases the CO2/N2 selectivity for the Pebax/ZIF-8 membranes compared to that of the pure Pebax membrane, and the highest CO2/N2 selectivity was 34.79 at 15 wt% ZIF-8. In addition, there was no significant change in the CO2/CH4 selectivity of the Pebax/ZIF-8 membranes. Therefore, CO2 permeability remarkably increases without sacrificing the gas selectivity, which is still beneficial for approaching the “Robeson upper-bound”.


image file: c6ra27221e-f10.tif
Fig. 10 Ideal selectivity of the pure Pebax membrane and Pebax/ZIF-8 membranes for CO2/N2 and CO2/CH4 as a function of ZIF-8 content.

3.4 Gas separation performance of the Pebax/ZIF-8/IL composite membranes

3.4.1 Effect of IL addition on the gas diffusivity and solubility coefficients. Considering the relatively high CO2 permeability and CO2/N2, CO2/CH4 selectivity, the Pebax/ZIF-8(15%)/[Bmim][NTf2] composite membranes with IL content varying from 0 to 80 wt% were prepared herein. The effect of IL addition on the diffusivity and solubility coefficients of N2, CH4, and CO2 for the Pebax/ZIF-8/IL membranes were investigated and are shown in Fig. 11.
image file: c6ra27221e-f11.tif
Fig. 11 (a) Diffusivity coefficients and (b) solubility coefficients of N2, CH4, and CO2 for the Pebax/ZIF-8(15%) membrane and Pebax/ZIF-8/IL membranes as a function of IL content.

The diffusivity coefficients of N2, CH4, and CO2 for the Pebax/ZIF-8/IL membranes dramatically increased compared to that of Pebax/ZIF-8(15%) membrane with the addition of IL, especially after 20 wt% IL content. IL acts as a low-molecular weight additive, leading to a more flexible structure and higher chain mobility, which can be concluded from DSC and SEM results. In addition, the decrease in the crystallinity of the Pebax/ZIF-8/IL membranes leads to a higher FFV.32 The high chain mobility and FFV facilitate gases diffusion leading to a higher gas diffusivity coefficient.32,34

N2, CH4, and CO2 diffusivity coefficients for the Pebax/ZIF-8/IL membranes fluctuate with the IL content varying from 0–20 wt% and there is a slight reduction in the CH4 diffusivity coefficients. SEM images show that the addition of IL fills the voids between the ZIF-8 particles and polymer, which will hinder the gas diffusion. Therefore, IL has two roles: the higher chain mobility and FFV of the prepared membranes facilitate gas diffusion, whereas a decrease in the number of voids between the ZIF-8 particles and polymer inhibits gas diffusion. Therefore, the reduction in the gas diffusivity coefficients appears to be more dependent on the blocking effect at a low IL content.

Fig. 11(b) shows that the CH4 and CO2 solubility coefficients of the Pebax/ZIF-8/IL membranes decrease with the IL addition compared to those of the Pebax/ZIF-8(15%) membrane, and there was no remarkable change in the N2 solubility coefficients. These results are mainly caused by the solubility of the pure IL. The solubility coefficient of the Pebax/ZIF-8(15%) membrane is 3.57 × 10−2 (cm3(STP) per (cm3 cm Hg)), and the solubility coefficient of the pure IL is 3.115 × 10−2 (cm3(STP) per (cm3 cm Hg)), as reported in the literature.40 The solubility of the pure IL is lower than that of the Pebax/ZIF-8(15%) membrane, resulting in a slight decrease in the CO2 solubility coefficients for the Pebax/ZIF-8/IL with the increasing IL content. This observation is similar to those for N2 and CH4.

3.4.2 Effect of IL addition on the gas permeability and selectivity. Fig. 12 shows that N2, CH4, and CO2 permeabilities for Pebax/ZIF-8/IL membranes are significantly enhanced compared to those of the Pebax/ZIF-8(15%) membrane with the addition of IL. For CO2, the permeability reached 231.4 barrer at an 80 wt% IL content, which is 111% higher than that of Pebax/ZIF-8(15%) membrane. The permeabilities of N2 and CH4 also increased by 174% and 145% compared to those of the Pebax/ZIF-8(15%) membrane. The enhancement in the permeability was attributed to the dramatic increase in the gas diffusivity coefficients. Therefore, IL increases the gas permeability of the Pebax/ZIF-8/IL membranes mainly by facilitating gas diffusion. Small fluctuations were permitted because of the fluctuations in the gas diffusivity coefficients with the IL content from 0–20 wt%.
image file: c6ra27221e-f12.tif
Fig. 12 Gas permeability of N2, CH4, and CO2 for the Pebax/ZIF-8(15%) membrane and Pebax/ZIF-8/IL membranes as a function of IL content.

Fig. 13 shows that the CO2/N2 selectivity of the Pebax/ZIF-8/IL membranes increases when the IL content is lower than 20 wt%, and the best CO2/N2 selectivity of the Pebax/ZIF-8/IL membranes is 42.07 at 10 wt% IL content. The addition of IL can improve the compatibility between the inorganic particles and polymer matrix. Therefore, the non-selective voids decrease and lead to a higher CO2/N2 selectivity of Pebax/ZIF-8/IL. However, the CO2/N2 selectivity of the Pebax/ZIF-8/IL membranes decreases at a high IL content (20–80 wt%). This was attributed to the intrinsically lower CO2/N2 selectivity of the IL itself. Furthermore, there was almost no change in the CO2/CH4 selectivity of the Pebax/ZIF-8/IL membranes.


image file: c6ra27221e-f13.tif
Fig. 13 Ideal selectivity of CO2/N2 and CO2/CH4 for the Pebax/ZIF-8(15%) membrane and Pebax/ZIF-8/IL membranes as a function of IL content.

To clearly display the gas separation performance of the prepared membranes, Robeson plots of the CO2/N2 performance are displayed in Fig. 14. The 2008 upper-bound of CO2/N2 is cited from the literature.41 In addition, the three-component composite membranes reported in other studies17,18,42,43 are also presented in Fig. 14. As a result, Pebax/ZIF/IL membranes in this study show comparable CO2/N2 separation performance and there is a significant increase in the CO2 permeability. The CO2 permeability of all the prepared membranes was in the following order: Pebax-ZIF(15%)-IL(80%) > Pebax-IL(80%) > Pebax-ZIF(15%) > pure Pebax membrane. Moreover, Pebax-ZIF(15%)-IL(10%) shows the highest CO2/N2 selectivity with a value of 42.07, which is much higher than that of the [Bmim][NTf2] supported membranes (19.68) reported in the literature.44 Compared to the Pebax/ZIF-8 and Pebax/IL composite membranes, the Pebax/ZIF-8/IL membranes exhibited superior CO2 separation performance. In addition, the Pebax/ZIF-8/IL membranes can be an effective approach to avoid IL leakage, which is a conventional problem for the supported ionic liquid membranes (SILMs). Therefore, the incorporation of ZIF-8 and [Bmim][NTf2] into the polymer matrix is a promising way to efficiently separate CO2.


image file: c6ra27221e-f14.tif
Fig. 14 Comparison of the membranes used in this study, SILMs,44 and the three-component MMMs reported in other studies17,18,42,43 for the CO2/N2 separation with the 2008 Robeson upper-bound.

4. Conclusions

Herein, a series of composite membranes with high gas transport properties enhanced by IL were developed. The results showed that the addition of IL can enhance the gas permeability of the Pebax/IL membranes, and the anions of ILs play a significant role in determining the gas permeability, which is similar to the principle of gas solubility in pure IL. Moreover, both the affinity of IL for the polymer and the inherent gas selectivity capacity of the IL influence the gas separation performance of the Pebax/IL membranes. The reduction in the polymer crystallinity and the formation of narrow voids by ZIF-8 facilitate CO2 diffusion. In addition, a decrease in the diffusivity coefficients for N2 and CH4 can be observed. The addition of IL can improve the compatibility between the inorganic particles and the polymer matrix, thus the non-selective voids decrease and lead to a higher CO2/N2 selectivity of the Pebax/ZIF-8/IL. High gas transport properties were obtained in the membranes with the addition of IL. This was attributed to the flexible structure and high FFV of the membranes with a decrease in the crystallinity, which promotes gas diffusion. The CO2 permeability of the Pebax/ZIF-8(15%)/IL(80%) composite membrane was 4.3 times higher than that of the pure Pebax membrane without sacrificing the CO2/N2 selectivity. Therefore, the three-component composite membranes containing IL, inorganic fillers, and organic polymer membranes with high gas transport properties can be a promising approach for the efficient separation of CO2.

Acknowledgements

This work was financially supported by the National Natural Science Fund for Distinguished Young Scholars (No. 21425625), the National Natural Science Foundation of China (No. 21506219, No. 51574215, No. 21606233), and the Corporation Program with State Key Laboratory of Organic-Inorganic Composites, Beijing University of Chemical Technology (No. oic-201601005).

Notes and references

  1. N. MacDowell, N. Florin, A. Buchard, J. Hallett, A. Galindo, G. Jackson, C. S. Adjiman, C. K. Williams, N. Shah and P. Fennell, Energy Environ. Sci., 2010, 3, 1645 CAS.
  2. S. D. Kenarsari, D. Yang, G. Jiang, S. Zhang, J. Wang, A. G. Russell, Q. Wei and M. Fan, RSC Adv., 2013, 3, 22739–22773 RSC.
  3. D. L. Gin and R. D. Noble, Science, 2011, 332, 674–676 CrossRef CAS PubMed.
  4. R. Khalilpour, K. Mumford, H. Zhai, A. Abbas, G. Stevens and E. S. Rubin, J. Cleaner Prod., 2015, 103, 286–300 CrossRef CAS.
  5. A. Kılıç, Ç. Atalay-Oral, A. Sirkecioğlu, Ş. B. Tantekin-Ersolmaz and M. G. Ahunbay, J. Membr. Sci., 2015, 489, 81–89 CrossRef.
  6. T. Rodenas, M. van Dalen, E. García-Pérez, P. Serra-Crespo, B. Zornoza, F. Kapteijn and J. Gascon, Adv. Funct. Mater., 2014, 24, 249–256 CrossRef CAS.
  7. T.-H. Bae and J. R. Long, Energy Environ. Sci., 2013, 6, 3565 CAS.
  8. L. B. J. Deng, S. J. Zeng, X. P. Zhang, Y. Nie, L. Y. Deng and S. J. Zhang, RSC Adv., 2016, 6, 45184–45192 RSC.
  9. H. Z. Chen, P. Li and T.-S. Chung, Int. J. Hydrogen Energy, 2012, 37, 11796–11804 CrossRef CAS.
  10. M. Yu, H. H. Funke, R. D. Noble and J. L. Falconer, J. Am. Chem. Soc., 2011, 133, 1748–1750 CrossRef CAS PubMed.
  11. P. K. Prajapati, A. M. Kansara and P. S. Singh, RSC Adv., 2016, 6, 88943–88953 RSC.
  12. A. F. Bushell, P. M. Budd, M. P. Attfield, J. T. Jones, T. Hasell, A. I. Cooper, P. Bernardo, F. Bazzarelli, G. Clarizia and J. C. Jansen, Angew. Chem., Int. Ed., 2013, 52, 1253–1256 CrossRef CAS PubMed.
  13. M. Rezakazemi, A. Ebadi Amooghin, M. M. Montazer-Rahmati, A. F. Ismail and T. Matsuura, Prog. Polym. Sci., 2014, 39, 817–861 CrossRef CAS.
  14. T. Rodenas, I. Luz, G. Prieto, B. Seoane, H. Miro, A. Corma, F. Kapteijn, F. X. Llabres i Xamena and J. Gascon, Nat. Mater., 2015, 14, 48–55 CrossRef CAS PubMed.
  15. Z. Lei, C. Dai and B. Chen, Chem. Rev., 2014, 114, 1289–1326 CrossRef CAS PubMed.
  16. Z. Dai, R. D. Noble, D. L. Gin, X. Zhang and L. Deng, J. Membr. Sci., 2016, 497, 1–20 CrossRef CAS.
  17. Y. C. Hudiono, T. K. Carlisle, A. L. LaFrate, D. L. Gin and R. D. Noble, J. Membr. Sci., 2011, 370, 141–148 CrossRef CAS.
  18. Y. C. Hudiono, T. K. Carlisle, J. E. Bara, Y. Zhang, D. L. Gin and R. D. Noble, J. Membr. Sci., 2010, 350, 117–123 CrossRef CAS.
  19. D. F. Mohshim, H. Mukhtar and Z. Man, Sep. Purif. Technol., 2014, 135, 252–258 CrossRef CAS.
  20. T. Khosravi and M. Omidkhah, RSC Adv., 2015, 5, 12849–12859 RSC.
  21. J. Lillepaerg, P. Georgopanos, T. Emmler and S. Shishatskiy, RSC Adv., 2016, 6, 11763–11772 RSC.
  22. S. Shahid, K. Nijmeijer, S. Nehache, I. Vankelecom, A. Deratani and D. Quemener, J. Membr. Sci., 2015, 492, 21–31 CrossRef CAS.
  23. S. Zhao, X. Cao, Z. Ma, Z. Wang, Z. Qiao, J. Wang and S. Wang, Ind. Eng. Chem. Res., 2015, 54, 5139–5148 CrossRef CAS.
  24. T. K. Carlisle, J. E. Bara, C. J. Gabriel, R. D. Noble and D. L. Gin, Ind. Eng. Chem. Res., 2008, 47, 7005–7012 CrossRef CAS.
  25. S. Wang, Y. Liu, S. Huang, H. Wu, Y. Li, Z. Tian and Z. Jiang, J. Membr. Sci., 2014, 460, 62–70 CrossRef CAS.
  26. M. J. C. Ordoñez, K. J. Balkus, J. P. Ferraris and I. H. Musselman, J. Membr. Sci., 2010, 361, 28–37 CrossRef.
  27. S. Kanehashi, M. Kishida, T. Kidesaki, R. Shindo, S. Sato, T. Miyakoshi and K. Nagai, J. Membr. Sci., 2013, 430, 211–222 CrossRef CAS.
  28. D. Zhao, J. Ren, H. Li, X. Li and M. Deng, J. Membr. Sci., 2014, 467, 41–47 CrossRef CAS.
  29. M. C. McCarthy, V. Varela-Guerrero, G. V. Barnett and H.-K. Jeong, Langmuir, 2010, 26, 14636–14641 CrossRef CAS PubMed.
  30. T. Zhou, L. Luo, S. Hu, S. Wang, R. Zhang, H. Wu, Z. Jiang, B. Wang and J. Yang, J. Membr. Sci., 2015, 489, 1–10 CrossRef CAS.
  31. H. Wu, X. Li, Y. Li, S. Wang, R. Guo, Z. Jiang, C. Wu, Q. Xin and X. Lu, J. Membr. Sci., 2014, 465, 78–90 CrossRef CAS.
  32. H. Rabiee, A. Ghadimi and T. Mohammadi, J. Membr. Sci., 2015, 476, 286–302 CrossRef CAS.
  33. S. Feng, J. Ren, Z. Li, H. Li, K. Hua, X. Li and M. Deng, Int. J. Greenhouse Gas Control, 2013, 19, 41–48 CrossRef CAS.
  34. A. Ghadimi, M. Amirilargani, T. Mohammadi, N. Kasiri and B. Sadatnia, J. Membr. Sci., 2014, 458, 14–26 CrossRef CAS.
  35. A. Car, C. Stropnik, W. Yave and K.-V. Peinemann, J. Membr. Sci., 2008, 307, 88–95 CrossRef CAS.
  36. R. Surya Murali, A. F. Ismail, M. A. Rahman and S. Sridhar, Sep. Purif. Technol., 2014, 129, 1–8 CrossRef CAS.
  37. M. C. McCarthy, V. Varela-Guerrero, G. V. Barnett and H.-K. Jeong, Langmuir, 2010, 26, 14636–14641 CrossRef CAS PubMed.
  38. H. Lin and B. D. Freeman, J. Mol. Struct., 2005, 739, 57–74 CrossRef CAS.
  39. H. Q. Lin and B. D. Freeman, Macromolecules, 2005, 38, 8394–8407 CrossRef CAS.
  40. J. E. Bara, T. K. Carlisle, C. J. Gabriel, D. Camper, A. Finotello, D. L. Gin and R. D. Noble, Ind. Eng. Chem. Res., 2009, 48, 2739–2751 CrossRef CAS.
  41. L. M. Robeson, J. Membr. Sci., 2008, 320, 390–400 CrossRef CAS.
  42. L. Hao, P. Li, T. Yang and T.-S. Chung, J. Membr. Sci., 2013, 436, 221–231 CrossRef CAS.
  43. R. Shindo, M. Kishida, H. Sawa, T. Kidesaki, S. Sato, S. Kanehashi and K. Nagai, J. Membr. Sci., 2014, 454, 330–338 CrossRef CAS.
  44. P. Scovazzo, J. Membr. Sci., 2009, 343, 199–211 CrossRef CAS.

Footnote

Electronic supplementary information (ESI) available. See DOI: 10.1039/c6ra27221e

This journal is © The Royal Society of Chemistry 2017