Jose A.
Carrasco
a,
Jorge
Romero
a,
María
Varela
b,
Frank
Hauke
c,
Gonzalo
Abellán
*ac,
Andreas
Hirsch
c and
Eugenio
Coronado
*a
aInstituto de Ciencia Molecular (ICMol), Universidad de Valencia, Catedrático José Beltrán 2, 46980, Paterna, Valencia, Spain. E-mail: gonzalo.abellan@fau.de
bUniversidad Complutense de Madrid, Dpt. Fisica Aplicada III & Instituto Pluridisciplinar, Madrid 28040, Spain
cDepartment of Chemistry and Pharmacy and Institute of Advanced Materials and Processes (ZMP), University Erlangen-Nürnberg, Henkestr. 42, 91054 Erlangen and Dr.-Mack Str. 81, 90762 Fürth, Germany
First published on 15th February 2016
Alkoxide-intercalated NiFe-layered double hydroxides were synthesized via the nonaqueous methanolic route. These nanoplatelets exhibit high crystalline quality as demonstrated by atomic resolution scanning transmission electron microscopy combined with electron energy-loss spectroscopy. Moreover, the presence of the alkoxide moieties has been unambiguously demonstrated by means of thermogravimetric analysis coupled to a mass spectrometer. These NiFe-LDHs can be exfoliated in water or organic solvents and processed into homogeneous ultra-thin films (<3 nm thick) with the assistance of O2-plasma. The study of their behaviour as water oxidation electrocatalysts has shown an outstanding performance at basic pHs (small overpotential of ca. 249 mV and Tafel slopes in the range of 52–55 mV per decade).
LDH can be formulated as [MII1−χMIIIχ(OH)2]χ+(An−)χ/n·mH2O, in which MII and MIII are divalent and trivalent metals, respectively (like MII = Mg2+, Zn2+, Ni2+, Co2+, and Fe2+ or MIII = Al3+, Fe3+, Co3+, Ni3+ or Cr3+), and An− is the interlayer anion which can be organic or inorganic and is placed between the cationic hydroxide sheets in order to compensate the excess of positive charge. One of the main features of these systems is their high chemical tunability, which allows them to be synthesized with different metallic compositions without altering their structure, leading to a wide range of properties. Moreover, the facile exfoliation of these LDH into monolayer nanosheets has boosted the attention paid to these materials.11
Among all the different possible compositions they exhibit, the combination of Ni and Fe (NiFe-LDHs) seems to be the most promising on the basis of its recent successful application as a highly efficient carbon monoxide (CO) oxidation catalyst,12 their excellent behaviour as electroactive material in the water photolysis,13–15 their use on high performance batteries16,17 or as catalytic precursors for the CVD synthesis of novel carbon nanoforms.18–21
The synthesis and exfoliation of pure NiFe-LDHs with high crystallinity and well-defined hexagonal shapes have remained elusive so far.22,23 Currently, there are two main routes for the synthesis of pure NiFe-LDHs that can be exfoliated into 2D nanosheets, namely the hydrothermal approach using urea as ammonium releasing reagent and triethanolamine as chelating reagent,23,24 and the use of anthraquinone-2-sulfate that favors the topochemical oxidation of the metals during the layer formation.25,26 These aqueous methodologies avoid the Fe oxidation, leading to NiFe-LDHs without spinel impurities.27 When it comes to non-aqueous routes Gardner et al. described a synthetic procedure to obtain nanometric alkoxide-intercalated Al-containing LDHs using alcohols as solvents.28,29 In this sense, we recently applied this method to synthesize pure CoFe-LDHs that can be exfoliated in water and exhibit excellent electrochemical properties.30
In the present work, we have extended this non-aqueous route for the synthesis of NiFe-LDHs, obtaining alkoxide-intercalated nanoplatelets that exhibit size-dependent magnetic properties. Furthermore, we have explored their exfoliation in water and developed their processing into ultra-thin films with homogeneous coverage. Finally, we have characterized their electrochemical behavior as OER electrocatalysts showing an outstanding performance in alkaline solution.
[Ni0.66Fe0.33(OH)1.55(OMe)0.45](Cl)0.33·1H2O: (C, H, N, calc.: 4.2, 2.8, 0; found: 4.2, 3.1, 0.1).
[Ni0.69Fe0.31(OH)2](CO3)0.155·0.5H2O: (C, H, N, calc.: 2.0, 3.2, 0; found: 2.0, 3.6, 0.3).
For the deposition of exfoliated platelets in water, 1 mg of the sample was dissolved in 10 mL of Milli-Q water and sonicated for 30 min. Then, two approaches were considered, drop casting and spin coating (5000 rpm) of the solution onto the previously cleaned and treated with O2 plasma SiO2-Si wafer. On the other hand, for a complete coverage of the substrate a different approach was followed.31 Typically, 10 mg of the NiFe-A LDHs were dissolved in a mixture of 20 mL of 1-BuOH and 10 mL of formamide in a covered flask. The solution was placed in an ultrasonic bath for 30 min. Then, the SiO2-Si substrate was submerged into the solution for 5 min, followed by 1 min in a solution of 1-BuOH to remove the excess of LDH platelets. Afterwards, the substrates were dried at 70 °C overnight and stored in vacuum.
The powdered materials were mixed with acetylene black and PVDF in a mass ratio of 80:10:10 in ethanol and deposited on a nickel foam electrode. The as-prepared nickel foam electrodes were dried overnight at 80 °C and pressed. Each working electrode contained about 0.25–0.5 mg of electroactive material and had a geometric surface area of about 1 cm2. The synthesis of the in situ grown films was performed by following the same experimental procedure described for NiFe-A but replacing the magnet used for the stirring with Ni foam leading to the direct growth of NiFe-A on this material.33 A typical three-electrode experimental cell equipped with a stainless steel plate having 4 cm2 of surface area as the counter electrode, and a Metrohm Ag/AgCl (3 M KCl) as the reference electrode was used for the electrochemical characterization of the working electrodes. All measurements were carried out with magnetic agitation and nitrogen bubbling.
The electrochemical properties were studied measuring the CV at different scan rates in 1 M KOH aqueous solutions. In addition, chronoamperometric studies were performed at a constant overpotential (j = 0.3 V), and chronopotentiometric studies at constant current densities of 5 and 10 mA cm−2. All potentials reported in this manuscript were converted to the RHE reference scale using E(RHE) = E(NHE) + 0.059 pH = E°(Ag/AgCl) + 0.197 V + 0.059 pH. The turnover frequency (TOF) values were calculated from the equation:
TOF = JA/4Fm |
The synthesis of the LDH phase was confirmed by X-ray powder diffraction (XRPD) analysis (Fig. 1A), showing the characteristic (110) doublet at around 60° in 2θ, and the main basal reflection (003) at around 2θ = 9–9.5°, providing a basal space of ca. 9.3 Å, in good agreement with the expected values for MeO-intercalated LDH.28 For the sake of comparison the XRPD spectrum of the NiFe-LDH obtained by hydrothermal approach (NiFe-HT) was also depicted (Fig. 1A), showing the (003) reflection at a 11.4° indicative of the presence of carbonate anions in the interlamellar space.20,23
The Fourier transform infrared spectra (FTIR) of NiFe-A and NiFe-HT are compared in Fig. 1B. There are two bands in the former case at ca. 2950 and 1070 cm−1, related to C–H and C–O stretching vibrations, respectively, which are absent in the carbonate-intercalated sample, supporting the presence of the alkoxide anion in the interlamellar space.34
FESEM measurements were carried out to unveil the morphology of both samples (Fig. 1C). NiFe-A depicts homogeneous lateral dimensions of around 110 nm, in clear contrast to NiFe-HT, which depicts micrometric sizes (see ESI 1 and 2† for additional FESEM images).24 It is worth to remark that, whereas the morphology of the NiFe-HT consists on well-defined hexagonal shapes, NiFe-A does not show this good definition, resulting into more irregular flakes.
Similar dimensions have been reported for the MgAl derivative by Gursky et al.,29 or conventional NiAl-HT.35 For CoFe-A synthesized with our non-aqueous method, values of ca. 20 nm were reported.30 EDAX mapping confirmed the expected 2:1 Ni:Fe ratio showing a homogeneous distribution of the two metals throughout the whole sample (Fig. 1E–G). Furthermore, elemental analysis, microanalysis, and thermogravimetric analysis of the sample allowed us to estimate the following molecular formula for NiFe-A: [Ni0.66Fe0.33(OH)1.55(OMe)0.45](Cl−)0.33·1H2O.
Direct information of the microstructure of the nanoplatelets can be obtained by aberration-corrected STEM-EELS. Fig. 2A shows a high angle annular dark field (HAADF) STEM image of a single NiFe-A flake. The platelet-like nanocrystal has a lateral dimension of ∼35 nm, the smaller size is related with the rupture of the flake after the sonication used for the preparation of the TEM grid. Fig. 2B depicts a high magnification atomic resolution image showing a high quality crystalline structure. In order to confirm the chemical composition of the sample, the corresponding EEL spectrum was obtained working at 80 kV and illuminating a crystal while scanning the electron beam in order to minimize the beam-induced damage. The O K, Fe L2,3 and Ni L2,3 edges are visible, near 530 eV, 708 eV, and 855 eV, respectively. The quantification of the spectra using the routine available in the Gatan Digital Micrograph software (and hydrogenic-white line cross-sections) yields a Ni:Fe atomic ratio of 1:(0.61 ± 0.09), in good agreement with EDAX microanalysis.
To provide further insight into the chemical nature of the intercalated species we have characterised, for the first time, the NiFe-LDH samples with thermogravimetric analysis coupled with a mass spectrometer (TG-MS) under an inert atmosphere of helium (Fig. 3). This powerful technique allows us to unambiguously identify the interlamellar anions, confirming the intercalation of the alkoxide groups.36 Analysis of NiFe-HT from room temperature to 500 °C revealed the presence of carbonate (CO2, m/z 44) with a continuous mass loss peaking at ca. 280 °C. With respect to the H2O (m/z 18), a first intense mass loss attributed to the weakly physisorbed water appeared between room temperature and ca. 180 °C, then a second and more intense mass loss takes place at around 274 °C and is correlated with the dehydroxylation of the layers as well as with the detachment of chemisorbed water present in the interlamellar space (Fig. 3A).36 In the case of NiFe-A the continuous MS enabled the allocation of the molecular fragments corresponding to the alkoxide moiety, m/z 31 and 32, at around 270 °C, a temperature remarkably higher than that of the pristine MeOH (ca. 65 °C). Interestingly, no signal of CO2 was detected till the appearance of a tiny peak centered at ca. 264 °C, indicative for the residual character of the carbonate contamination in the alkoxide-intercalated samples as recently observed for other hybrid MgAl- and ZnAl-LDHs.36 Its worth to remark that the CO2 signal of NiFe-A at higher temperature is also related with the combustion of the organic anions (Fig. 3B).
One of the main features of LDH is their ability to be exfoliated in appropriate solvents.11 In the case of the alkoxide-intercalated LDH is also possible to perform the exfoliation in water. Indeed, by suspending 1 mg of LDH in 10 mL of Milli-Q water and sonicating during 30 min, a clear colloidal suspension showing Tyndall-Faraday effect can be prepared. Dynamic light scattering measurements provided an average hydrodynamic diameter of ca. 140 nm in excellent agreement with the FESEM studies (Fig. 4). The exfoliation and further deposition of the NiFe-A sample on SiO2-Si substrates was also confirmed via AFM measurements. We firstly performed a typical drop casting of the NiFe-A water suspension observing the accretion of the platelets into clusters of ca. 10–20 nm in thickness (Fig. 4A and B). This situation can be overcome by spin coating the same solution at 5000 rpm (two times) lowering the thickness to ca. 2.5 nm (Fig. 4C).
The processability of LDH into thin films is one of the most rapidly growing areas in this field, as the large-scale correct disposition of the LDH platelets would facilitate their application in energy storage and conversion devices.20,37 Along this front, we checked the formation of continuous thin films by physical deposition. The first attempts with the water suspensions were unsatisfactory due to an inhomogeneous coverage even after using O2-plasma cleaning for the activation of the substrates (Fig. 4). To face this challenge we used a solvent mixture of 1-buthanol and formamide, following a slight modification of the method reported by Jung et al.31 including O2-plasma activation. As seen in Fig. 5, complete coverage of the substrate was achieved, with lateral sizes of ca. 50–100 nm for the platelets and small RMS values of 0.83 nm. The average height of the coverage is 2.67 nm, revealing a highly homogeneous film. The scratch of the film gave us an approximate thickness value, resulting in ca. 1 nm (average of the measurement in different points), very close to that expected for a monolayer. This film is remarkably thinner than that previously synthesized by in situ growth of the NiFe-LDH on glass substrates (ca. 138–170 nm).20 A control experiment on a cleaned substrate including its RMS value is depicted in the ESI 3.† The role exerted by the oxygen plasma is crucial. Indeed, control experiments without using the O2-plasma revealed poor deposition of the LDH, with higher thickness values that might be attributed to some agglomeration of the platelets (Fig. 5D). The plasma treatment allows us to activate the silicon substrate with negative charges,38,39 leading to a better bonding with the positive LDH cationic sheets, and resulting in a homogeneous and large coverage (additional images can be seen in ESI 4†).
The chemical integrity of the resulting films was confirmed by XPS. Fig. 5E and F shows the high-resolution Ni 2p and Fe 2p XPS spectra of the film confirming the presence of Ni(II) and Fe(III) in the samples. The Ni 2p spectrum exhibit two main peaks at 855 and 873 eV, related to the spin–orbit splitting of the Ni (2p3/2) and Ni (2p1/2), respectively. In the case of Fe 2p, two peaks are centred at binding energies of 713 and 726 eV, indicative for Fe (2p3/2) and Fe (2p1/2), respectively. These binding energy values are in good agreement with those expected for NiFe-LDH phases.14,20,40 Our new synthetic route represents a straightforward way for the preparation of homogeneous ultrathin films of NiFe-LDH.
The overall magnetism of a LDH system is controlled by two main contributions.10 On the one hand the intralayer magnetic superexchange interactions between metallic centres through the hydroxyl (OH–) bridges across the cationic sheets. On the other hand, the less intense dipolar interactions, which take place in the space between the magnetic LDH layers (interlayer nature). In our specific case, NiFe-LDHs behave as low-temperature ferrimagnets due to the coexistence between ferromagnetic Ni–OH–Ni superexchange interactions along with antiferromagnetic Ni–OH–Fe and Fe–OH–Fe interactions.20,24,27,30,41 All magnetic measurements were carried out in a SQUID with freshly prepared powdered samples. The main magnetic data and parameters have been summarized in Table 1, including NiFe-HT24 and CoFe-A30 for comparative purposes. The DC susceptibility measurements (χM) depict a sharp increase near 50 K, reaching a maximum value of 0.63 emu mol−1 at 4.5 K, indicative of cooperative magnetic interactions (Fig. 6A). On the other hand, the thermal variation of χMT decreases from a value of 1.93 emu K mol−1 at room temperature to 1.86 emu K mol−1 at 70 K. After that, χMT exhibits a sharp increase upon cooling to its maximum value of 4 emu K mol−1 at 8.1 K, followed by an abrupt decrease to 1.23 emu K mol−1 at 2 K (Fig. 6A). Fitting the DC data to the Curie–Weiss law above 50 K gives rise to a Curie constant (C) of 1.95 emu K mol−1 consistent with that expected for the spin only value of a magnetically diluted combination of Ni2+ (S = 1) and Fe3+ (S = 5/2) ions (Table 1).24 Moreover, the positive value (4.74 K) of the Weiss constant (θ) is indicative for the predominance of ferromagnetic interactions throughout the layers, although its value is remarkably smaller than in the NiFe-HT. Field cooled and zero field cooled (FC/ZFC) measurements allowed us to extract both blocking and irreversible temperatures, resulting in TB = 4.8 K and Tirr = 5 K, respectively (Fig. 6B). Hysteresis loop were also recorded at 2 and 20 K – below and above the blocking temperature (Fig. 6C), confirming the presence of spontaneous magnetization at low temperatures. The coercive field increases as long as we decrease the temperature, as expected, with a Hc of 690 Oe at 2 K and 30 Oe for 20 K. These Hc values are always lower than 1000 Oe, concluding that this NiFe-A LDH is a soft magnet, in good agreement with what is found for the CoFe-A.24,30 On the other hand, micrometric NiFe-HT depicted a higher coercive field of ca. 3600 Oe for the 2:1 ratio, as well as a much higher irreversible temperature (15.1 K) pointing towards superparamagnetic behaviour of the NiFe-A due to the dramatic decrease in the particle size.24
Sample | χT rt (emu K mol−1) | C so (emu K mol−1) | C (emu K mol−1) | θ (K) | T irr (K) | T M (K) | T Hys (K) | M S (μB) | H c (Oe) | Δ/kB (K) | ν 0 (Hz) | ϕ | Ref. |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
a χT rt value at room temperature; expected spin-only value of the Curie constant (Cso); experimental Curie constant (C); Weiss constant (θ); temperature of the divergence of the ZFC and FC magnetic susceptibility (Tirr); temperature for the onset of spontaneous magnetization extracted from the χ′′M plot (TM); measured hysteresis temperature (THys); saturation magnetization (MS); coercive field (HCoer); energy barrier (Δ/kB) and frequency factor (ν0), resulting from the fitting of the magnetic susceptibility to the Arrhenius law; Mydosh parameter (ϕ). S(Ni2+) = 1, S(Fe3+) = 5/2. | |||||||||||||
NiFe-A | 1.93 | 2.10 | 1.95 | 4.74 | 5.0 | 7.8 | 2; 20 | 0.97; 0.74 | 690; 30 | 275.7 | 9.1 × 1024 | 0.043 | This work |
CoFe-A | 2.48 | 2.50 | 2.57 | −14.69 | 4.8 | 7.0 | 2.0 | 0.98 | 402 | 116.9 | 3.8 × 1014 | 0.063 | 30 |
NiFe-HT | 2.29 | 2.10 | 2.56 | 29.11 | 15.1 | 16.8 | 2.0 | 0.76 | 3600 | 1381.5 | 2.01 × 1040 | 0.021 | 24 |
AC dynamic susceptibility measurements in the presence of an external field of 3.95 Oe oscillating at different frequencies in the 1–10000 Hz interval were carried out in order to confirm the cooperative magnetism in the sample (Fig. 6D). In both cases, the in-phase (χ′M) and the out-of-phase (χ′′M) signals exhibit a defined peak at low temperatures.
From the out-of-phase signal we can extract the temperature for the onset of the spontaneous magnetization (TM), set as the point where χ′′M ≠ 0. For the NiFe-A TM = 7.8 K, remarkably lower than that observed for NiFe-HT (TM = 16.8 K), which is indicative of size effects.42 As the experimental ratio is 2:1 between Ni:Fe (χ = 0.33), the Fe3+ clustering cannot be avoided, as previously demonstrated by Mössbauer spectroscopy for NiFe-HT, leading to a glassy magnetic behaviour.24 Along with that, both signals χ′M and χ′′M exhibit a significant frequency dependence. The frequency dependence of the χ′′M maxima can be estimated with the calculation of the frequency shift parameters defined by Mydosh:43,44
Φ = ΔTmax/[TmaxΔ(logν)] | (1) |
For NiFe-A, the value Φ ≈ 0.043 is higher than that observed for canonical spin glasses (0.005–0.018)43 and within the range of values associated to spin glass-like materials (0.06–0.08). Notice that nanosized NiAl-, CoAl-45 and CoFe-LDHs,30 exhibit Φ values in this range, in line with the expected size effects. In contrast, in NiFe-HT Φ is in the range of values associated close to canonical spin glasses (Φ ≈ 0.021).24 Further information of the spin relaxation in these materials can be obtained by fitting the frequency dependence of χ′′M to both an Arrhenius law and a 3D critical scaling law.
The Arrhenius law for a thermally activated process is described by the following equation:
ν = ν0exp(−Ea/kBT) | (2) |
For NiFe-A a fitting of the frequency dependence of χ′′M to this law gives a value for energy barrier of Ea/kB = 276 K, which can be ascribed to the presence of a superparamagnetic behaviour,43 in clear contrast to the NiFe-HT sample that exhibits a higher value of ca. 1400 K. These results highlight the crucial role of the nanometric size and low dimensionality of these LDH systems in sharp contrast with the micrometric ones.46
Finally, we have fitted the frequency dependence of χ′′M to the 3D critical scaling law for spin dynamics,47,48 which is described by the following equation:
τ = τ0[Tg/(Tg/Tmax − Tg)]zν | (3) |
A similar behaviour was reported by Layrac et al. for different magnetic LDHs intercalated with cyano-bridged coordination polymers.47 For NiFe-HT, the best fit (see ESI 5†) was found for Tg = 14.9 K, τ0 = 2.55 × 10−7 s and zν = 2.7.48 In overall, these results indicate a spin-glass like behaviour for these NiFe-LDHs, with superparamagnetic effects in the NiFe-A derivative arising from the nanometric size of the samples.44,47
To demonstrate the applicability of these novel NiFe-LDHs in the field of energy storage and conversion, we have investigated their performance as OER electrocatalysts for the multi-electron reaction: 4OH− ↔ O2 + 2H2O + 4e−, in alkaline media.49–51 Beyond other compositions, the catalysts containing earth-abundant Ni and Fe cations are among the most efficient reported so far.52,53 Along this front, the performance exhibited by NiFe-LDH and its corresponding carbon hybrids have been studied.14,15,26,54,55–57
The electrocatalytic OER activity of NiFe-LDH was tested in a basic medium (1 M KOH) in a standard three-electrode cell. For comparative purposes we have prepared working electrodes consisting on NiFe-A and NiFe-HT, as well as commercial IrO2 catalyst as a reference, using powdered samples coated on Ni-foam collectors. Moreover, to overcome the intrinsic insulating behaviour of LDH, avoid the detachment of the active material due to the exfoliation in water and in order to improve their catalytic performance and stability, we have directly grown 3D porous films of NiFe-A on Ni-foam – hereinafter: NiFe-A-NiFoam – following a modified procedure previously described in the literature (see ESI 6†).13,33 The cyclic voltammetry at different scan rates of NiFe-A (Fig. 7A) reveals the presence of a redox peak around 1.35 V vs. RHE, that can be assigned to the Ni(II)/Ni(III or IV) redox processes, probably related with the transformation between Ni1−xFex(OH)2 and Ni1−xFexOOH (see ESI 7† for additional CVs of the other the samples).14,33,58 Moreover, the anodic wave of the NiFe-A catalyst is nearly merged with the catalytic wave but a distinct cathodic feature is evident, in excellent accordance with previous reports (see ESI 7† for pristine Ni-foam blank experiments and additional CVs of the other sample).58,59
The catalytic materials were measured by linear sweep voltammetry, showing the lowest onset potential for the NiFe-A-NiFoam (1.51 V vs. RHE), followed by the NiFe-HT and the pristine NiFe-A (Fig. 7B and ESI 7†). Different parameters were calculated to quantify the improvements of activity: the overpotential (η) at different current densities (5, 10 and 30 mA cm−2), the current density (j) at η = 300 mV and the Tafel slopes (the performance of the different samples have been summarized in ESI 8†). The current density of 10 mA cm−2 was chosen because it represents the current density from a device with 12% solar to hydrogen efficiency, considered as a realistic measure of the catalytic activity.15
As presented in Fig. 7C, an overpotential of ca. 0.249 V is required at j = 10 mA cm−2 for NiFe-A-NiFoam, a value much smaller than that of NiFe-HT (more than 0.32 V) or NiFe-A (0.34 V) and similar to that previously published by Lu and co-workers.33 In Fig. 7D it can be seen that the overpotential is decreased by 60–80 mV by growing the LDH directly on the Ni-foam. The excellent catalytic activity of the as-synthesized NiFe-LDHs is also reflected in the Tafel slopes, showing values in the range of 52–55 mV per decade, much smaller that that exhibited by the commercial IrO2 (we should indicate that the Tafel slopes not solely reflect the kinetic information of water oxidation but a combined process of redox reactions and OER).
To further evaluate their electrocatalytic activity, the values of the turnover frequency (TOF) of the powdered samples were calculated by assuming that all the transition metal ions in the catalysts are contributing to the reaction, which also confirm that NiFe-A has the highest TOF of 0.01 s−1 at an overpotential of 0.3 V, nearly of NiFe-HT (0.007). It is worth to keep in mind that these TOF values compete favourably with those recently reported for others NiFe-LDHs.26,33
The stability and durability of the NiFe-A powdered catalyst was tested at constant current densities j of 5 and 10 mA cm−2 and with a constant overpotential of η 300 mV for 1000 s. In Fig. 7G, we can see a very high stability in both cases. When increasing the current density from 5 to 10 mA cm−2 the overpotential correspondingly increases to ca. 0.03 V (see ESI 7† for additional measurements). These results are in good accordance with NiFe-LDH nanosheets synthesized using the topochemical approach having the same composition (Ni:Fe 2:1).26 It is worth to remark here that the spin-glass magnetic behaviour exhibited by these NiFe-LDH can be correlated to the presence of Fe-clustering, and this may play a role in their OER behaviour. Indeed, as recently pointed out by M. A. Oliver-Tolentino et al. the superexchange interactions could exert a big influence in the electrocatalytic activity.60 When compared to Ni(OH)2, the more complex local environment around Ni–O pairs in NiFe-LDHs plays a crucial role in the OER activity, increasing the NiOOH conductivity >30-fold. In fact, Fe exerts a partial-charge transfer activation effect on the Ni atoms, improving the catalytic activity.58 Moreover, operando Mössbauer spectroscopic studies demonstrated the exclusive formation of Fe4+ in NiFe, but not in Fe-only catalysts, as a result of the stabilizing effect of the local NiOOH lattice, most probably on the edges, corners or defects.59 In any case, the role of the particle size and defect sites in the OER behaviour of NiFe-LDH catalysts remains an open question. These results illustrate the great potential exhibited by NiFe-A as a cheap electrocatalyst for the OER, and opens the door for its hybridization with organic counterparts like graphene or carbon nanotubes in order to further improve its electrochemical performance.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c6qi00009f |
This journal is © the Partner Organisations 2016 |