Shichun
Li
ab,
Shuwen
Yu
ac,
Sean M.
Collins
bd,
Duncan N.
Johnstone
b,
Christopher W.
Ashling
b,
Adam F.
Sapnik
b,
Philip A.
Chater
e,
Dean S.
Keeble
e,
Lauren N.
McHugh
b,
Paul A.
Midgley
b,
David. A.
Keen
f and
Thomas D.
Bennett
*b
aInstitute of Chemical Materials, China Academy of Engineering Physics, Mianyang 621900, P. R. China
bDepartment of Materials Science and Metallurgy, University of Cambridge, 27 Charles Babbage Road, Cambridge CB3 0FS, UK. E-mail: tdb35@cam.ac.uk
cXiamen Institute of Rare Earth Materials, Haixi Institute, Chinese Academy of Sciences, Xiamen 361021, P. R. China
dSchool of Chemical and Process Engineering and School of Chemistry, University of Leeds, LS2 9JT, UK
eDiamond House, Harwell Science & Innovation Campus, Diamond Light Source, Ltd., Didcot, Oxfordshire OX11 0DE, UK
fISIS Facility, Rutherford Appleton Laboratory, Harwell Campus, Didcot, Oxon OX11 0QX, UK
First published on 28th August 2020
Metal–organic framework crystal–glass composite (MOF CGC) materials consist of a crystalline MOF embedded within a MOF–glass matrix. In this work, a new synthetic route to these materials is demonstrated through the preparation of two ZIF-62 glass-based CGCs, one with crystalline ZIF-67 and the other with crystalline UiO-66. Previous attempts to form these CGCs failed due to the high processing temperatures involved in heating above the melting point of ZIF-62. Annealing of the ZIF-62 glass above the glass transition with each MOF however leads to stable CGC formation at lower temperatures. The reduction in processing temperatures will enable the formation of a greatly expanded range of MOF CGCs.
A further complication results from the susceptibility of MOFs to chemical degradation.9 Zeolitic imidazolate frameworks (ZIFs) for example, have been shown to be highly prone to degradation via acid catalysed Zn–N bond hydrolysis, which causes progressive collapse of the crystal structure accompanied by a reduction in internal surface area.11,12 Other MOFs that are relatively stable in acid, such as UiO-66 and MOF-545, are unstable to basic conditions.13
Various strategies have been proposed to enhance the processability and stability of crystalline MOFs, including modulated synthesis and post-synthetic modification,13 sol–gel processing,14 and fabrication of MOF based composites such as mixed matrix membranes (MMMs).15,16 In this latter example, crystalline MOF particles are dispersed in a polymer matrix,7,17 though poor interfacial compatibility between the polymer and crystalline MOF component leads to several related issues such as the formation of interfacial mesoporous voids and aggregation of the MOF component.18,19 Matrices possessing both good processability and compatibility with crystalline MOFs are therefore highly sought after.
The recent discovery of MOFs which form glasses20–22 opens up possible opportunities to solve processability and compatibility issues, by using a MOF–glass as a binder. ZIFs are a subset of MOFs containing tetrahedral metal ions, which are linked by imidazolate (Im, C3H3N2−) derived bidentate ligands and have structures closely related to zeolitic silica polymorphs. In particular, ZIF-62, [Zn(Im)1.75(bIm)0.25] (bIm, benzimidazolate, C7H5N2−), has been shown to form a glass of identical composition (referred to as agZIF-62), by quenching from the liquid at ca. 437 °C in an argon (Ar) atmosphere. Bulk, transparent and bubble-free forms have previously been prepared by remelting and annealing agZIF-62 above its glass transition temperature (Tg) of 318 °C.23 The absence of recrystallisation of the glass upon reheating, or slow cooling, is ascribed to the volume collapse from open crystalline to dense glass.24
We have previously fabricated MOF crystal–glass composites (MOF CGCs), in which crystalline MIL-53 [Al(OH)(O2C–C6H4–CO2)] or UiO-66 [Zr6O4(OH)4(O2C–C6H4–CO2)6] were dispersed within an agZIF-62 matrix.25 The composites were fabricated by heating a mixture of crystalline ZIF-62 and MIL-53 or UiO-66 under Ar to 450 °C, i.e. above the melting point (Tm) of ZIF-62, before cooling back down to room temperature. The crystallinity was preserved in MIL-53 CGCs but UiO-66 was found to undergo partial decomposition due to the high temperatures involved in composite formation.25
MOF CGCs may have promise in applications in gas adsorption, membrane separation, and photocatalysis, though the range of MOF CGCs which may be synthesized by this high-temperature route is however limited at present. Major problems are that the high processing temperatures result in (i) the partial or complete thermal decomposition of the crystalline component, or (ii) the dissolution of chemically compatible ZIFs in the liquid at high temperature (i.e. flux melting).
Motivated to develop lower temperature methods for the synthesis of MOF CGCs, we present here a new strategy for MOF CGC fabrication. Specifically, mixtures of pre-synthesized agZIF-62 and crystalline MOF were annealed at 400 °C, a temperature which is sufficiently above Tg (318 °C) but still below Tm (ca. 440 °C) such that ZIF-62 can be considered within its supercooled liquid regime and the glass has effectively melted.
To highlight the advantages of this method of preparation, ZIF-67 (the isostructural cobalt(II) analogue of ZIF-8), and UiO-66 were chosen as the crystalline components. The former has been reported to undergo flux-melting within the liquid state of ZIF-62,26,27 whilst the latter undergoes partial decomposition.25 Thus far, stable MOF crystal-glass composites have therefore not been formed from either ZIF-67 or UiO-66. These two crystalline MOFs therefore represent ideal candidates on which to attempt to form MOF CGCs using this new processing route.
Here, we use powder X-ray diffraction and X-ray total scattering to show the retention of crystallinity among the crystalline component of MOF–CGCs upon annealing with agZIF-62 above its Tg. Morphology and component distribution within the CGCs are characterized using scanning electron microscopy (SEM), scanning transmission electron microscopy (STEM), X-ray energy dispersive spectroscopy (EDS), and scanning electron diffraction (SED). Thermomechanical analysis (TMA) and chemical stability testing demonstrated improved thermo-mechanical stability compared to the pure crystalline precursors.
The pellets formed prior to heating are referred to as (‘MOF’)(agZIF-62)(X/Y) in keeping with prior literature, where X and Y indicate the percentage by mass of the crystalline and glass components respectively. For example, a non-heat treated pellet of 80 wt% ZIF-67 and 20 wt% agZIF-62 is referred to as (ZIF-67)(agZIF-62)(80/20).
MOF CGCs were then fabricated by heating the pelleted mixtures at 400 °C for 5 hours under Ar to remelt the agZIF-62 component (Fig. 1a). The CGCs obtained upon cooling are referred to as (‘MOF’)X(agZIF-62)Y. For example, a CGC with 80 wt% ZIF-67 and 20 wt% agZIF-62 is referred to as (ZIF-67)0.8(agZIF-62)0.2. The preservation of crystallinity in both ZIF-67 and UiO-66 was confirmed by X-ray diffraction (Fig. 1b, S2, and Table S1†), in contrast to previous efforts at CGC fabrication using these systems.25,26 The samples of (ZIF-67)0.8(agZIF-62)0.2 and (UiO-66)0.8(agZIF-62)0.2 (Fig. 1c and d) were macroscopic solid pieces, demonstrating the bulk samples obtained using this approach.
Synchrotron X-ray total scattering measurements were performed on (i) pure samples of agZIF-62, UiO-66 and ZIF-67, (ii) the physical mixtures after pressing, though prior to remelting; and (iii) the three MOF CGCs formed after melting (Fig. 2 and S3†). The structure factors, S(Q), for ZIF-67, UiO-66, physical mixtures and CGCs contain extensive Bragg scattering as expected. The intensity of Bragg scattering from ZIF-67 decreased in the pelletized mixture, consistent with reported partial pressure induced amorphization,32 and then again after CGC formation (Fig. 2a, b and S3†). The results are consistent with those in Fig. 1b, confirming retention of crystallinity within the CGCs, though this appears slightly reduced in the MOF–CGCs compared to the pressed physical mixtures. The pair distribution functions (PDFs), D(r), of agZIF-62, ZIF-67, (ZIF-67)(agZIF-62)(80/20) and (ZIF-67)0.8(agZIF-62)0.2 are similar below 7.5 Å (Fig. 2c, e, S3c†), though contain subtle differences such as the position of peak i.26 Long range oscillations beyond 8 Å persist in the CGC sample, as expected, though weaken with decreasing weight fraction of ZIF-67 in CGCs (Fig. S3c†). The PDFs of the UiO-66 CGCs display characteristic peaks of both agZIF-62 and UiO-66, (Fig. 2d, e).25 Like those for the ZIF-67 CGC, long range correlations in the CGCs (ascribed to Zr–Zr correlations) also weaken with decreasing weight fraction of UiO-66 (Fig. S3d†).
The surfaces of (UiO-66)(agZIF-62)(X/Y) and (UiO-66)X(agZIF-62)Y were far less uniform, consistent with the lower pressures applied for pelletisation being insufficient to force close contact between the viscous ZIF-62 liquid and UiO-66 particles during remelting. Cracks at the boundaries between agZIF-62 and UiO-66 in both (UiO-66)(agZIF-62)(X/Y) and (UiO-66)X(agZIF-62)Y were located in representative EDS mappings (Fig. 3, S5, S7†). These were not observed between ZIF-67 and agZIF-62, suggesting better interfacial contact for ZIF-67 CGCs.
The (ZIF-67)0.5(ZIF-62)0.5 sample was ground into a powder and characterized using scanning transmission electron microscopy (STEM) to investigate the CGC microstructure (Fig. 4). Scanning Electron Diffraction (SED) was used to map the number of detected Bragg diffraction peaks measured at each probe position as the electron probe was scanned across the sample to reveal the location of crystalline phases in the MOF-CGCs, as shown in Fig. 4c and d. These are in effect qualitative maps of crystallinity as determined by the presence of Bragg peaks in crystalline domains and absence of Bragg peaks in non-crystalline regions (Fig. S8†).
The maps of the crystalline regions demonstrate close contact between crystalline and non-crystalline regions. Comparison with compositional maps showing the distribution of metal centres, obtained via STEM-EDS mapping of the same particles and shown in Fig. 4e and f, confirms that the crystalline regions, indicated with red arrows in Fig. 4b, d and f, correspond to cobalt-rich regions, as expected for ZIF-67. Conversely, amorphous regions, indicated with blue arrows in Fig. 4a, c and e, also correspond to the presence of Zn-centres, consistent with the agZIF-62 domains in (ZIF-67)0.5(ZIF-62)0.5.
Fig. 5 Gas sorption. N2 gas isotherms at 77 K of (a) ZIF-67 series, and (b) UiO-66 series. Solid circles represent adsorption, and hollow circles represent desorption. |
In contrast, CGC formation resulted in only a slight decrease in gas sorption capacity in both cases (Fig. 5). For example, BET surface areas decreased from 981 m2 g−1 (ZIF-67)(agZIF-62)(80/20) to 901 m2 g−1 (ZIF-67)0.8(agZIF-62)0.2, and from 683 m2 g−1 to 632 m2 g−1 from (UiO-66)(agZIF-62)(80/20) to (UiO-66)0.8(agZIF-62)0.2.
As expected, the gas sorption quantity of CGCs increases with the weight fraction of MOF crystals in the CGCs (Fig. S11†). The decrease in BET surface area of the CGC relative to that of the mixture for ZIF-67 is non-linear with the weight fraction of the ZIF-67 (Fig. S11c†). This implies a strong interaction between ZIF-67 and agZIF-62 in the CGC, causing partial collapse or blockage of the pores of ZIF-67. The equivalent BET surface area decrease for UiO-66 on CGC formation is approximately proportional to the weight fraction of UiO-66.
Here, the linear thermal expansion of a sample of agZIF-62 was measured for the first time, alongside the expansivities of pellets of MOF crystals, physical mixtures and CGCs (Fig. 6 and S12†). The glass sample, agZIF-62, was found to possess an average coefficient of thermal expansion (CTE) of 35 × 10−6 K−1 between 35 °C and 275 °C. This is much higher than that of silica-based inorganic glasses (0.59–8.5 × 10−6 K−1), and lower than that of most polymers (45–200 × 10−6 K−1), although we note that some polymers have a lower CTE, such as Kapton (20 × 10−6 K−1).39,40 This intermediate thermal expansion is perhaps expected given the inorganic–organic bonding within the system, but is nevertheless a beautiful example of the hybrid nature of the physical properties of bulk MOF systems, alongside the hybrid chemical properties often touted. A softening point, equivalent to the glass transition, was noted at 320 °C (Fig. 6a).
Fig. 6 Thermo-mechanical properties. Linear thermal expansion of (a) agZIF-62 and (b) ZIF-67 series measured by TMA. |
The pellets of physical mixtures and CGCs (Fig. 6b, S12†) display a lower thermal expansivity than agZIF-62 over 100 °C, which is in agreement with the non-uniform nature of the sample and the presence of macroscale defects within the bulk solid. The absence of deformation (inferred from the scatter in data points) at low temperatures of the (ZIF-67)0.8(agZIF-62)0.2 sample is mainly attributed to the strong interaction between agZIF-62 and ZIF-67 in the CGC. However, in the case of UiO-66, deformation of (UiO-66)0.8(agZIF-62)0.2 was inferred from the start of measurement (Fig. S12†), which is caused by the dehydroxlyation of UiO-66 during remelting.
Specifically, the mass loss per surface area of agZIF-62 was measured after soaking a pellet of agZIF-62 in a given aqueous solution at room temperature for 7 days (Fig. S13†), which is a widely used method for assessing the stability of glasses.40 No obvious weight loss of agZIF-62 was observed in the pH range of 5–12 (Fig. 7a), indicating agZIF-62 is stable in this pH range. Apparent corrosion on the surface was however observed by SEM at pHs lower than 5, and higher than 12 (Fig. 7a), though no re-crystallization was found after the soaking experiments (Fig. S14†). The stability of agZIF-62, i.e. stable in all but very basic conditions and unstable in strongly acidic conditions, is consistent with previous observations on crystalline ZIFs, which is caused by the relatively high pKa values of azoles.9
The chemical stability of CGCs was judged by comparing the N2 adsorption quantity, e.g. BET surface area (Fig. 7b, S15†), XRD pattern (Fig. S16†), and SEM images (Fig. S17†) before, and after soaking them in aqueous solutions. Pellets of pure MOF crystals were also investigated for comparison. The samples containing ZIF-67 were soaked in aqueous acid at pH 5 for 7 days, and UiO-66 containing samples were soaked in an aqueous base at pH 12 for 7 days. A dramatic decrease in the BET surface area from 1269 m2 g−1 to 365 m2 g−1 was observed for a pellet of pure ZIF-67 after soaking, whilst only a slight decrease in BET surface area from 901 m2 g−1 to 805 m2 g−1 was found in the case of (ZIF-67)0.8(ZIF-62)0.2 after soaking (Fig. 7b).
Hysteresis in the N2 gas isotherm of pellet of ZIF-67 (Fig. S15a†) is broadly consistent with the degradation inferred by decreases in the intensity of Bragg peaks in the XRD pattern (Fig. S16a†), and the sheet-like morphology on the surface observed by SEM (Fig. S17a†). This is also consistent with the literature and is associated with a reduction in surface area.11,12 Strikingly, the degradation of ZIF-67 in the CGC was far less pronounced than that in the pellet of pure ZIF-67, indicating that (ZIF-67)0.8(ZIF-62)0.2 possesses better stability in aqueous acid than the pellet of pure ZIF-67. This may be attributed to the lower water uptake of (ZIF-67)0.8(ZIF-62)0.2 than that of the pellet of pure ZIF-67 (Fig. S18a†), which slows down the rate of hydrolysis of Co–N coordination bonds. The lower water uptake of (ZIF-67)0.8(agZIF-62)0.2 is attributed to the strongly hydrophobic nature of agZIF-62 and the unique interfacial structure between agZIF-62 and ZIF-67 in the CGC.
In the case of UiO-66, however, a severe decrease in BET surface area was found for (UiO-66)0.8(ZIF-62)0.2 after soaking, in comparison to a pellet of pure UiO-66 (Fig. 7b). This decrease in surface area is consistent with the decrease in intensity of Bragg peaks in the corresponding XRD pattern (Fig. S16b†). This may be caused by the dehydroxylation of UiO-66 in the CGC during remelting that leads to defects in UiO-66. The presence of existing defects in UiO-66 in the CGC favour further defect formation,12 leading to amorphization, although (UiO-66)0.8(agZIF-62)0.2 possesses lower water uptake than the pellet of UiO-66.
The lower temperatures also lead to better preservation of porosity within the formed CGCs toward N2. The thermal expansion of a MOF–glass was investigated for the first time and found to be intermediate between inorganic and organic polymers – showing that it is not just the chemical properties of MOFs which are hybrid in nature. A significant improvement in thermo-mechanical properties and chemical stabilities of the CGCs compared with pellets of the pure crystalline MOFs was noted, and bulk monolithic CGCs of the type fabricated here may show promising applications in membrane separation and photocatalysis.
The bulk agZIF-62 pellet was fabricated by remelting of agZIF-62 powders.23 Specifically, 150 mg of agZIF-62 powder was pressed into a pellet with a diameter of 13 mm under 10 tons for 1 min, and then heated under Ar to 400 °C at a ramping rate of 20 °C min−1 and held for 5 hours in a tube furnace, followed by naturally cooling to room temperature.
The bulk ZIF-67 pellet was fabricated by pressing 150 mg evacuated ZIF-67 powder under 10 tons for 1 min. The bulk UiO-66 pellets were fabricated by pressing 150 mg evacuated UiO-66 powder under 2 tons and 10 tons at first, though the loss of porosity was significant due to the bond breakage of UiO-66 after compression. Thus, the bulk UiO-66 pellet was fabricated by pressing 150 mg of unevacuated UiO-66 powder under 2 tons for 1 min.
A series of MOF CGCs with different mass fraction, e.g. 20 wt%, 50 wt% and 80 wt%, of ZIF-67 or UiO-66 were prepared. The MOF crystal and agZIF-62 powders were mixed by grinding in a mortar for 5 min. Subsequently, the 150 mg mixture was pressed at 10 tons (for ZIF-62 containing mixture) or 2 tons (for UiO-66 containing mixture) for 1 min, and then heated under Ar to 400 °C at a ramping rate of 20 °C min−1 and held for 5 hour in a tube furnace, followed by naturally cooling to room temperature.
SED data were processed using an open source Python library, pyxem-0.10.0,46 to find diffraction peaks in every measured diffraction pattern using a difference of Gaussians method, which involves subtracting a blurred version of the diffraction pattern from a less blurred version of the diffraction pattern. EDS data were processed using the open-source HyperSpy Python library to produce maps for each X-ray emission line of interest (Zr Kα, Zn Kα), which were extracted by integrating an energy window and background subtracted by linear interpolation from adjacent regions of the spectrum without other X-ray peaks present.47
Footnote |
† Electronic supplementary information (ESI) available: X-ray diffraction, electron microscopy, gas sorption and chemical stability measurements. See DOI: 10.1039/d0sc04008h |
This journal is © The Royal Society of Chemistry 2020 |